MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Incoloy 807 Nickel Alloy
Categories: Metal; Nonferrous Metal; Nickel Alloy

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 8.32 g/cc0.301 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Ultimate  220 MPa
@Temperature 870 °C
31900 psi
@Temperature 1600 °F
Bar
 350 MPa
@Temperature 760 °C
50800 psi
@Temperature 1400 °F
Bar
 440 MPa
@Temperature 650 °C
63800 psi
@Temperature 1200 °F
Bar
 470 MPa
@Temperature 540 °C
68200 psi
@Temperature 1000 °F
Bar
 655 MPa
@Temperature 21.0 °C
95000 psi
@Temperature 69.8 °F
Bar
Tensile Strength, Yield  185 MPa
@Strain 0.2 %,
Temperature 870 °C
26800 psi
@Strain 0.2 %,
Temperature 1600 °F
Bar
 225 MPa
@Strain 0.2 %,
Temperature 760 °C
32600 psi
@Strain 0.2 %,
Temperature 1400 °F
Bar
 240 MPa
@Strain 0.2 %,
Temperature 650 °C
34800 psi
@Strain 0.2 %,
Temperature 1200 °F
Bar
 255 MPa
@Strain 0.2 %,
Temperature 540 °C
37000 psi
@Strain 0.2 %,
Temperature 1000 °F
Bar
 380 MPa
@Strain 0.2 %,
Temperature 21.0 °C
55100 psi
@Strain 0.2 %,
Temperature 69.8 °F
Bar
Elongation at Break  34 %
@Temperature 760 °C
34 %
@Temperature 1400 °F
Bar
 35 %
@Temperature 650 °C
35 %
@Temperature 1200 °F
Bar
 40 %
@Temperature 540 °C
40 %
@Temperature 1000 °F
Bar
 48 %
@Temperature 21.0 °C
48 %
@Temperature 69.8 °F
Bar
 71 %
@Temperature 870 °C
71 %
@Temperature 1600 °F
Bar
Rupture Strength  19.0 MPa
@Temperature 980 °C,
Time 3.60e+6 sec
2760 psi
@Temperature 1800 °F,
Time 1000 hour
Bar
 43.0 MPa
@Temperature 870 °C,
Time 3.60e+6 sec
6240 psi
@Temperature 1600 °F,
Time 1000 hour
Bar
 105 MPa
@Temperature 760 °C,
Time 3.60e+6 sec
15200 psi
@Temperature 1400 °F,
Time 1000 hour
Bar
Modulus of Elasticity  128 GPa
@Temperature 870 °C
18600 ksi
@Temperature 1600 °F
 137 GPa
@Temperature 760 °C
19900 ksi
@Temperature 1400 °F
 146 GPa
@Temperature 650 °C
21200 ksi
@Temperature 1200 °F
 155 GPa
@Temperature 540 °C
22500 ksi
@Temperature 1000 °F
 184 GPa
@Temperature 21.0 °C
26700 ksi
@Temperature 69.8 °F
 
Thermal PropertiesMetricEnglishComments
CTE, linear  15.2 µm/m-°C
@Temperature 538 °C
8.44 µin/in-°F
@Temperature 1000 °F
 17.6 µm/m-°C
@Temperature 871 °C
9.78 µin/in-°F
@Temperature 1600 °F
Melting Point 1275 - 1355 °C2327 - 2471 °F
Solidus 1275 °C2327 °F
Liquidus 1355 °C2471 °F
 
Component Elements PropertiesMetricEnglishComments
Carbon, C 0.050 %0.050 %
Chromium, Cr 20.5 %20.5 %
Cobalt, Co 8.0 %8.0 %
Iron, Fe 25 %25 %
Manganese, Mn 0.50 %0.50 %
Molybdenum, Mo 0.10 %0.10 %
Nickel, Ni 40 %40 %
Silicon, Si 0.40 %0.40 %
Titanium, Ti 0.30 %0.30 %
Tungsten, W 5.0 %5.0 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Special Metals INCONEL® 625LCF® Nickel Superalloy (UNS N06626) Annealed + 20% Cold Work
Inconel 587 Nickel Alloy
Latrobe MP35N® Alloy
Sandvik Bioline F562/F562LTi Wire
Special Metals INCOLOY® alloy 908

NZ987 / 170616

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.