MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Dow SPECTRIM™ HH 390 Reaction Moldable Polymer  (discontinued **)
Categories: Polymer; Thermoset; Polyurethane, TS

Material Notes:

Information provided by Dow

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.26 g/ccASTM D792
Filler Content 20 %
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength, Ultimate 4346 psiperpendicular; ASTM D638
 4962 psiparallel; ASTM D638
Elongation at Break 52.7 %parallel; ASTM D638
 74.1 %perpendicular; ASTM D638
Flexural Modulus 150000 psiperpendicular; ASTM D790
 273000 psiparallel; ASTM D790
Izod Impact, Notched 2.06 ft-lb/inASTM D256
Dart Drop, Total Energy 2.504 JMax Load; ASTM D3763
 12.65 JASTM D3763
Instrumented Impact Total Energy 20.4 JASTM D3763
Instrumented Impact Energy at Peak 6.50 JEnergy at Max load; ASTM D3763
 
Thermal PropertiesOriginal ValueComments
CTE, linear 26.7 µin/in-°F
@Temperature -40.0 °C
ASTM D696
 28.9 µin/in-°F
@Temperature 66.1 °C
ASTM D696
 30.6 µin/in-°F
@Temperature 121 °C
ASTM D696
CTE, linear, Transverse to Flow 71.3 µin/in-°F
@Temperature -40.0 °C
ASTM D696
 78.2 µin/in-°F
@Temperature 66.1 °C
ASTM D696
 81.8 µin/in-°F
@Temperature 121 °C
ASTM D696
Deflection Temperature at 0.46 MPa (66 psi) 400 °FASTM D648

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Covestro Baydur® GS PIR A Polyurethane
Covestro Baydur® GS PIR B Polyurethane
BCC Products BC 8165 Urethane Casting
Covestro Baytec® OCS 080D Polyurethane
Covestro Prism® CM-200 Polyurethane Solid RIM, MDI-based 2-Component Liquid System

PDOW1434 / 30652

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.