MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Toyobo GLAMIDE® T-422VOR Nylon-6
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 6 (PA6); Nylon 6, 20% Mineral Filled

Material Notes: GLAMIDE® is very tough and exhibits high abrasion resistance. It has a high melting point and heat resistance, has well-balanced proportions of mechanical properties, performs self-distinguishing and a specific grade approved as UL94V-0 class is provided, and it exhibits excellent chemical resistance and oil resistance. Grade T-422VOR is a flame resistant, aromatic, and mineral reinforced Nylon-6. It is of halogen origin.

23

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.56 g/ccAbsolute Drying; ASTM-D792
Filler Content 23 %
Water Absorption 0.50 %Absolute Drying; ASTM-D570
Moisture Absorption at Equilibrium 1.8 %Absolute Drying; ASTM-D570
Linear Mold Shrinkage 0.0010 - 0.0020 cm/cm
@Thickness 1.00 mm
Absolute Drying
 0.0030 - 0.0060 cm/cm
@Thickness 3.00 mm
Absolute Drying
Melt Flow 20 g/10 min
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell R 118Absolute Drying; ASTM-D785
Tensile Strength, Ultimate 24.0 MPa
@Temperature 80.0 °C
Practical Use (Water Absorption 1.8%); ASTM-D638
 28.0 MPa
@Temperature 80.0 °C
Absolute Drying; ASTM-D638
 38.0 MPa
@Temperature 23.0 °C
Practical Use (Water Absorption 1.8%); ASTM-D638
 51.0 MPa
@Temperature 23.0 °C
Absolute Drying; ASTM-D638
 61.0 MPa
@Temperature -40.0 °C
Practical Use (Water Absorption 1.8%); ASTM-D638
 65.0 MPa
@Temperature -40.0 °C
Absolute Drying; ASTM-D638
Elongation at Break 1.5 %Absolute Drying; ASTM-D638
 4.5 %Practical Use (Water Absorption 1.8%); ASTM-D638
Flexural Strength 38.0 MPa
@Temperature 80.0 °C
Practical Use (Water Absorption 1.8%); ASTM-D790
 50.0 MPa
@Temperature 80.0 °C
Absolute Drying; ASTM-D790
 63.0 MPa
@Temperature 23.0 °C
Practical Use (Water Absorption 1.8%); ASTM-D790
 90.0 MPa
@Temperature 23.0 °C
Absolute Drying; ASTM-D790
 104 MPa
@Temperature -40.0 °C
Practical Use (Water Absorption 1.8%); ASTM-D790
 110 MPa
@Temperature -40.0 °C
Absolute Drying; ASTM-D790
Flexural Modulus 1.20 GPa
@Temperature 80.0 °C
Practical Use (Water Absorption 1.8%); ASTM-D790
 3.40 GPa
@Temperature 80.0 °C
Absolute Drying; ASTM-D790
 4.40 GPa
@Temperature 23.0 °C
Practical Use (Water Absorption 1.8%); ASTM-D790
 6.10 GPa
@Temperature 23.0 °C
Absolute Drying; ASTM-D790
 6.40 GPa
@Temperature -40.0 °C
Practical Use (Water Absorption 1.8%); ASTM-D790
 7.20 GPa
@Temperature -40.0 °C
Absolute Drying; ASTM-D790
Compressive Strength 45.0 MPaPractical Use (Water Absorption 1.8%); ASTM-D695
 62.0 MPaAbsolute Drying; ASTM-D695
Izod Impact, Notched 30.0 J/m
@Temperature -40.0 °C
Absolute Drying; ASTM-D256
 40.0 J/m
@Temperature 23.0 °C
Absolute Drying; ASTM-D256
 45.0 J/m
@Temperature -40.0 °C
Practical Use (Water Absorption 1.8%); ASTM-D256
 70.0 J/m
@Temperature 23.0 °C
Practical Use (Water Absorption 1.8%); ASTM-D256
Taber Abrasion, mg/1000 Cycles 32CS-17, Absolute Drying; ASTM-D1044
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 1.00e+8 - 1.00e+9 ohm-cmPractical Use (Water Absorption 1.8%); ASTM-D257
 1.00e+12 ohm-cmAbsolute Drying; ASTM-D257
Dielectric Strength 20.0 kV/mm
@Thickness 2.00 mm
Practical Use (Water Absorption 1.8%); ASTM-D149
 29.0 kV/mm
@Thickness 2.00 mm
Absolute Drying; ASTM-D149
Arc Resistance 15 secPractical Use (Water Absorption 1.8%); ASTM-D495
 25 secAbsolute Drying; ASTM-D495
Comparative Tracking Index 350 VIEC Method
 
Thermal PropertiesOriginal ValueComments
CTE, linear 42.0 µm/m-°CAbsolute Drying; ASTM-D696
Deflection Temperature at 0.46 MPa (66 psi) 205 °CAbsolute Drying; ASTM-D648
Deflection Temperature at 1.8 MPa (264 psi) 160 °CAbsolute Drying; ASTM-D648
Flammability, UL94 V-0
 
Processing PropertiesOriginal ValueComments
Melt Temperature 250 - 285 °C
Mold Temperature 60.0 °C
Injection Pressure 40.0 - 60.0 MPa

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Toyobo GLAMIDE® T-402FR Nylon-6
Toyobo GLAMIDE® T-808-02 Nylon-6
Toyobo GLAMIDE® T-521 Nylon-6
Toyobo GLAMIDE® TY-791GT 6T-Nylon
Toyobo GLAMIDE® T-402 Nylon-6

PTOY943 / 107494

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.