MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Covestro Texin® 1209 Thermoplastic Polyurethanes (TPU)
Categories: Polymer; Thermoplastic; Polyurethane, TP

Material Notes: Characterization: Texin 1209 resin is an aromatic polyether-based thermoplastic polyurethane; it can be processed by injection molding or extrusion.

Properties / Applications: Texin 1209 resin is characterized by very good hydrolysis resistance, good low temperature flexibility, resiliency and impact strength, high moisture vapor transmission rates and is plasticizer free. Texin 1209 natural color resin complies with FDA food-contact regulations 21 CFR 177.1680 (Polyurethane Resins) and 177.2600 (Rubber Articles Intended for Repeated Use), subject to the limitations of these and any other applicable regulations. Applications include soft touch over-molding, roof linings, seals, membranes, films, rigid/flexible composite systems and sport shoe soles. As with any product, use of Texin 1209 resin in a given application must be tested (including but not limited to field testing) in advance by the user to determine suitability.

Information provided by Covestro

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.07 g/ccASTM D792
Linear Mold Shrinkage, Flow 0.0080 cm/cm
@Thickness 2.54 mm
ASTM D955
Linear Mold Shrinkage, Transverse 0.0080 cm/cm
@Thickness 2.54 mm
ASTM D955
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 70ASTM D2240
Tensile Strength at Break 25.5 MPaASTM D412
Tensile Stress at Strain 3.40 MPa
@Strain 100 %
ASTM D412
 5.20 MPa
@Strain 300 %
ASTM D412
Elongation at Break 770 %ASTM D412
Flexural Modulus 14.5 MPa
@Temperature 23.0 °C
ASTM D790
 106.9 MPa
@Temperature -30.0 °C
ASTM D790
Resilience 68[%], Bayshore; ASTM D2632
Tear Strength 60.5 kN/mDie C; ASTM D624
Taber Abrasion, mg/1000 Cycles 7.0
@Load 1.00 kg
[mg] Loss, H-18; ASTM D3489
Compression Set 11 %
@Temperature 23.0 °C,
Time 79200 sec
postcured; ASTM D395-B
 30 %
@Temperature 70.0 °C,
Time 79200 sec
postcured; ASTM D395-B
 
Thermal PropertiesOriginal ValueComments
Vicat Softening Point 75.0 °CRate A; ASTM D1525
Glass Transition Temp, Tg -57.0 °C
 
Processing PropertiesOriginal ValueComments
Rear Barrel Temperature 182 - 193 °CInjection
 182 - 199 °CExtrusion
Middle Barrel Temperature 182 - 204 °CExtrusion
 188 - 199 °CInjection
Front Barrel Temperature 182 - 204 °CExtrusion
 188 - 199 °CInjection
Nozzle Temperature 191 - 202 °CInjection
Die Temperature 188 - 204 °CExtrusion
Melt Temperature 188 - 199 °CInjection
 191 - 240 °CExtrusion
Mold Temperature 16.0 - 38.0 °CInjection
Injection Pressure 6000 - 15000 psiInjection
Back Pressure <= 200 psiInjection
Cushion <= 0.125 inInjection
 
Compliance PropertiesOriginal ValueComments
FDA Yes

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Covestro Texin® RxT70A Thermoplastic Polyurethanes (TPU)
Covestro Texin® 970 U Thermoplastic Polyurethanes (TPU)
Covestro Texin® 270 Thermoplastic Polyurethanes (TPU)
Covestro Texin® 1210 Thermoplastic Polyurethanes (TPU)
Covestro Texin® 245 Thermoplastic Polyurethanes (TPU)

PCOVEST0988 / 202771

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.