MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Overview of materials for Polyphenylene Sulfide (PPS), Unreinforced, Extruded
Categories: Polymer; Thermoplastic; Polyphenylene Sulfide (PPS); Polyphenylene Sulfide (PPS), Unreinforced, Extruded

Material Notes: This property data is a summary of similar materials in the MatWeb database for the category "Polyphenylene Sulfide (PPS), Unreinforced, Extruded". Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.

Vendors: Ensinger High Performance Plastics withstand severe environments, resist harsh chemicals, and perform well in extreme temperatures. They offer weight savings that have potential to drive lower cost systems.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 1.29 - 1.43 g/ccAverage value: 1.34 g/cc Grade Count:15
Water Absorption at Saturation 0.0100 - 0.0900 %Average value: 0.0352 % Grade Count:9
Melt Flow 12.0 - 130 g/10 minAverage value: 73.0 g/10 min Grade Count:4
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell M 82.0 - 118Average value: 94.3 Grade Count:7
Hardness, Shore D 80.0 - 84.0Average value: 81.2 Grade Count:5
Tensile Strength, Ultimate 55.0 - 359 MPaAverage value: 116 MPa Grade Count:14
Elongation at Break 2.00 - 40.0 %Average value: 15.7 % Grade Count:13
Elongation at Yield 8.00 - 12.0 %Average value: 9.50 % Grade Count:8
Modulus of Elasticity 2.60 - 6.21 GPaAverage value: 4.19 GPa Grade Count:6
Flexural Yield Strength 100 - 170 MPaAverage value: 129 MPa Grade Count:10
Flexural Modulus 2.50 - 5.52 GPaAverage value: 4.15 GPa Grade Count:7
Compressive Yield Strength 21.0 - 122 MPaAverage value: 58.4 MPa Grade Count:5
Shear Strength 62.0 MPaAverage value: 62.0 MPa Grade Count:4
Izod Impact, Notched (ISO) 2.00 - 30.0 kJ/m²Average value: 11.4 kJ/m² Grade Count:4
Charpy Impact, Notched 0.200 J/cm² - NBAverage value: 0.840 J/cm² Grade Count:6
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 1.00e+14 - 4.50e+16 ohm-cmAverage value: 7.69e+15 ohm-cm Grade Count:9
Surface Resistance 1.00e+14 - 1.00e+16 ohmAverage value: 2.69e+15 ohm Grade Count:8
Insulation Resistance 1.00e+13 - 1.00e+13 ohm
@Temperature 90.0 - 90.0 °C
Average value: 1.00e+13 ohm Grade Count:1
Dielectric Constant 2.70 - 3.60Average value: 3.28 Grade Count:9
Dielectric Strength 14.2 - 44.7 kV/mmAverage value: 22.8 kV/mm Grade Count:11
Dissipation Factor 0.00130 - 0.00500Average value: 0.00218 Grade Count:7
 
Thermal PropertiesOriginal ValueComments
CTE, linear 30.0 - 80.0 µm/m-°CAverage value: 55.6 µm/m-°C Grade Count:10
 12.0 - 145 µm/m-°C
@Temperature 100 - 200 °C
Average value: 67.4 µm/m-°C Grade Count:7
CTE, linear, Transverse to Flow 90.0 - 90.0 µm/m-°C
@Temperature 100 - 200 °C
Average value: 90.0 µm/m-°C Grade Count:1
Thermal Conductivity 0.200 - 0.349 W/m-KAverage value: 0.297 W/m-K Grade Count:8
Melting Point 280 - 285 °CAverage value: 282 °C Grade Count:7
Maximum Service Temperature, Air 170 - 260 °CAverage value: 203 °C Grade Count:8
Deflection Temperature at 1.8 MPa (264 psi) 95.0 - 260 °CAverage value: 155 °C Grade Count:15
Minimum Service Temperature, Air -50.0 - -20.0 °CAverage value: -40.0 °C Grade Count:5
Glass Transition Temp, Tg 88.0 - 220 °CAverage value: 155 °C Grade Count:6
Flammability, UL94 V-0Grade Count:4
 
Processing PropertiesOriginal ValueComments
Melt Temperature 290 - 330 °CAverage value: 309 °C Grade Count:3

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Overview of materials for Polyetheretherketone, Unreinforced
Overview of materials for Polyetherimide (PEI)
Overview of materials for Polyphenylene Sulfide (PPS); Molded
Overview of materials for Polyetherketoneketone (PEKK), Unreinforced
Overview of materials for Polytetrafluoroethylene (PTFE), Extruded

O4501 / 78335

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.