MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Sunoco Ultraclear™ TR3350UC Random Polypropylene Copolymer  (discontinued **)
Categories: Polymer; Thermoplastic; Polypropylene (PP); Polypropylene Copolymer

Material Notes: Maximum See-Through Clarity, Minimal Haze; Superior Color Stability, Process Stability, and Gloss; Low Odor, High Melt Flow Market Segment: Consumer Products and Cups & Containers

Suggested Uses: Reusable Food Containers, Housewares, Fast-Cycle Injection Molding, Packaging

Ultraclear™ polypropylene resin offers unsurpassed clarity and performance, up to 50% improvement in haze over standard clarified products. It offers substitution opportunities versus more expensive resins such as PET, PVC, PC or PS.

Braskem acquired Sunoco Chemicals polypropylene product line in 2010.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Melt Flow 35 g/10 min
@Load 2.16 kg,
Temperature 230 °C
35 g/10 min
@Load 4.76 lb,
Temperature 446 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Yield 31.7 MPa4600 psi2 in/min; ASTM D638
Elongation at Yield 13 %13 %2 in/min; ASTM D638
Flexural Modulus, 1% Secant 1170 MPa170000 psi0.05 in/min; ASTM D790A
Izod Impact, Notched NBNBASTM D256A
 
Optical PropertiesMetricEnglishComments
Haze 5.0 %
@Thickness 1.27 mm
5.0 %
@Thickness 0.0500 in
Disc; ASTM D1003
Transmission, Visible 80 %80 %thickness unknown

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Wacker Vinnol® E 15/40 A TF Vinyl Chloride Copolymer
Geon® Performance Solutions 130 Series 136 Polyvinyl Chloride Copolymer (PVC Copolymer)
Braskem TR3350UC Random Copolymer Polypropylene
Geon® Performance Solutions 130 Series 137 Polyvinyl Chloride Copolymer (PVC Copolymer)
Geon® Performance Solutions 130 Series 138 Polyvinyl Chloride Copolymer (PVC Copolymer)

PSUN891 / 87592

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.