MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

(Viewing data as-entered. Click here to return)
Aluminum 3003-O
Categories: Metal; Nonferrous Metal; Aluminum Alloy; 3000 Series Aluminum Alloy

Material Notes: Good weldability/formability and very good corrosion resistance lead to applications such as food and chemical handling, tanks, trim, litho sheet, pressure vessels, and piping.

Data points with the AA note have been provided by the Aluminum Association, Inc. and are NOT FOR DESIGN.

Composition Notes:
Composition information provided by the Aluminum Association and is not for design.

Key Words: UNS A93003; ISO AlMn1Cu; Aluminium 3003-O; AA3003-O; Al3003-O
Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 2.73 g/ccAA; Typical
 
Mechanical PropertiesOriginal ValueComments
Hardness, Brinell 28AA; Typical; 500 g load; 10 mm ball
Tensile Strength, Ultimate 16.0 ksiAA; Typical
 18.0 MPa
@Temperature 400 °C
 29.0 MPa
@Temperature 300 °C
 60.0 MPa
@Temperature 200 °C
 90.0 MPa
@Temperature 100 °C
 110 MPa
@Temperature 25.0 °C
 115 MPa
@Temperature -30.0 °C
 150 MPa
@Temperature -100 °C
 230 MPa
@Temperature -200 °C
 97.0 - 130 MPa
@Thickness 0.152 - 76.2 mm
Tensile Strength, Yield 6.00 ksiAA; Typical
 12.0 MPa
@Temperature 400 °C
 17.0 MPa
@Temperature 300 °C
 30.0 MPa
@Temperature 200 °C
 38.0 MPa
@Temperature 100 °C
 41.0 MPa
@Temperature 25.0 °C
 45.0 MPa
@Temperature -30.0 °C
 52.0 MPa
@Temperature -100 °C
 60.0 MPa
@Temperature -200 °C
 >= 34.0 MPa
@Thickness 0.152 - 76.2 mm
Elongation at Break 40 %
@Temperature 25.0 °C
 41 %
@Temperature -30.0 °C
 43 %
@Temperature -100 °C
 43 %
@Temperature 100 °C
 46 %
@Temperature -200 °C
 60 %
@Temperature 200 °C
 70 %
@Temperature 300 °C
 75 %
@Temperature 400 °C
 14 - 25 %
@Thickness 0.152 - 76.2 mm
 30 %
@Thickness 1.59 mm
AA; Typical
 40 %
@Diameter 12.7 mm
AA; Typical
Modulus of Elasticity 10000 ksiAA; Typical; Average of tension and compression. Compression modulus is about 2% greater than tensile modulus.
Notched Tensile Strength 110 MPa2.5 cm width x 0.16 cm thick side-notched specimen, Kt = 17.
Ultimate Bearing Strength 207 MPaEdge distance/pin diameter = 2.0
Bearing Yield Strength 83.0 MPaEdge distance/pin diameter = 2.0
Poissons Ratio 0.33
Fatigue Strength 7000 psi
@# of Cycles 5.00e+8
completely reversed stress; RR Moore machine/specimen
Machinability 10 %0-100 Scale of Aluminum Alloys
Shear Modulus 25.0 GPa
Shear Strength 11.0 ksiAA; Typical
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 21.0 ohm-cir-mil/ft
@Temperature 20.0 °C
AA; Typical
Magnetic Susceptibility 8.0e-7cgs/g at 25ºC
 
Thermal PropertiesOriginal ValueComments
CTE, linear 12.9 µin/in-°F
@Temperature 20.0 - 100 °C
AA; Typical; average over range
 21.5 µm/m-°C
@Temperature -50.0 - 20.0 °C
 24.1 µm/m-°C
@Temperature 20.0 - 200 °C
 25.1 µm/m-°C
@Temperature 20.0 - 300 °C
Specific Heat Capacity 0.893 J/g-°C
Thermal Conductivity 1340 BTU-in/hr-ft²-°FAA; Typical at 77°F
Melting Point 1190 - 1210 °FAA; Typical range based on typical composition for wrought products >= 1/4 in. thickness
Solidus 1190 °FAA; Typical
Liquidus 1210 °FAA; Typical
 
Processing PropertiesOriginal ValueComments
Annealing Temperature 775 °FCommercial practice: 750 to 1100°F, higher temperatures used only for flash annealing.
 
Component Elements PropertiesOriginal ValueComments
Aluminum, Al 96.7 - 99 %As remainder
Copper, Cu 0.05 - 0.20 %
Iron, Fe <= 0.70 %
Manganese, Mn 1.0 - 1.5 %
Other, each <= 0.05 %
Other, total <= 0.15 %
Silicon, Si <= 0.60 %
Zinc, Zn <= 0.10 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Aluminum 3003-H14
Aluminum 3003-H12
Aluminum 3003-H18
Alclad Aluminum 3003-O
Aluminum 6061-T6; 6061-T651

MA3003O / 8985

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.