MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Toyobo GLAMIDE® T-422VOR Nylon-6
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 6 (PA6); Nylon 6, 20% Mineral Filled

Material Notes: GLAMIDE® is very tough and exhibits high abrasion resistance. It has a high melting point and heat resistance, has well-balanced proportions of mechanical properties, performs self-distinguishing and a specific grade approved as UL94V-0 class is provided, and it exhibits excellent chemical resistance and oil resistance. Grade T-422VOR is a flame resistant, aromatic, and mineral reinforced Nylon-6. It is of halogen origin.

23

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.56 g/cc1.56 g/ccAbsolute Drying; ASTM-D792
Filler Content 23 %23 %
Water Absorption 0.50 %0.50 %Absolute Drying; ASTM-D570
Moisture Absorption at Equilibrium 1.8 %1.8 %Absolute Drying; ASTM-D570
Linear Mold Shrinkage  0.0010 - 0.0020 cm/cm
@Thickness 1.00 mm
0.0010 - 0.0020 in/in
@Thickness 0.0394 in
Absolute Drying
 0.0030 - 0.0060 cm/cm
@Thickness 3.00 mm
0.0030 - 0.0060 in/in
@Thickness 0.118 in
Absolute Drying
Melt Flow 20 g/10 min20 g/10 min
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell R 118118Absolute Drying; ASTM-D785
Tensile Strength, Ultimate  24.0 MPa
@Temperature 80.0 °C
3480 psi
@Temperature 176 °F
Practical Use (Water Absorption 1.8%); ASTM-D638
 28.0 MPa
@Temperature 80.0 °C
4060 psi
@Temperature 176 °F
Absolute Drying; ASTM-D638
 38.0 MPa
@Temperature 23.0 °C
5510 psi
@Temperature 73.4 °F
Practical Use (Water Absorption 1.8%); ASTM-D638
 51.0 MPa
@Temperature 23.0 °C
7400 psi
@Temperature 73.4 °F
Absolute Drying; ASTM-D638
 61.0 MPa
@Temperature -40.0 °C
8850 psi
@Temperature -40.0 °F
Practical Use (Water Absorption 1.8%); ASTM-D638
 65.0 MPa
@Temperature -40.0 °C
9430 psi
@Temperature -40.0 °F
Absolute Drying; ASTM-D638
Elongation at Break 1.5 %1.5 %Absolute Drying; ASTM-D638
 4.5 %4.5 %Practical Use (Water Absorption 1.8%); ASTM-D638
Flexural Strength  38.0 MPa
@Temperature 80.0 °C
5510 psi
@Temperature 176 °F
Practical Use (Water Absorption 1.8%); ASTM-D790
 50.0 MPa
@Temperature 80.0 °C
7250 psi
@Temperature 176 °F
Absolute Drying; ASTM-D790
 63.0 MPa
@Temperature 23.0 °C
9140 psi
@Temperature 73.4 °F
Practical Use (Water Absorption 1.8%); ASTM-D790
 90.0 MPa
@Temperature 23.0 °C
13100 psi
@Temperature 73.4 °F
Absolute Drying; ASTM-D790
 104 MPa
@Temperature -40.0 °C
15100 psi
@Temperature -40.0 °F
Practical Use (Water Absorption 1.8%); ASTM-D790
 110 MPa
@Temperature -40.0 °C
16000 psi
@Temperature -40.0 °F
Absolute Drying; ASTM-D790
Flexural Modulus  1.20 GPa
@Temperature 80.0 °C
174 ksi
@Temperature 176 °F
Practical Use (Water Absorption 1.8%); ASTM-D790
 3.40 GPa
@Temperature 80.0 °C
493 ksi
@Temperature 176 °F
Absolute Drying; ASTM-D790
 4.40 GPa
@Temperature 23.0 °C
638 ksi
@Temperature 73.4 °F
Practical Use (Water Absorption 1.8%); ASTM-D790
 6.10 GPa
@Temperature 23.0 °C
885 ksi
@Temperature 73.4 °F
Absolute Drying; ASTM-D790
 6.40 GPa
@Temperature -40.0 °C
928 ksi
@Temperature -40.0 °F
Practical Use (Water Absorption 1.8%); ASTM-D790
 7.20 GPa
@Temperature -40.0 °C
1040 ksi
@Temperature -40.0 °F
Absolute Drying; ASTM-D790
Compressive Strength 45.0 MPa6530 psiPractical Use (Water Absorption 1.8%); ASTM-D695
 62.0 MPa8990 psiAbsolute Drying; ASTM-D695
Izod Impact, Notched  0.300 J/cm
@Temperature -40.0 °C
0.562 ft-lb/in
@Temperature -40.0 °F
Absolute Drying; ASTM-D256
 0.400 J/cm
@Temperature 23.0 °C
0.749 ft-lb/in
@Temperature 73.4 °F
Absolute Drying; ASTM-D256
 0.450 J/cm
@Temperature -40.0 °C
0.843 ft-lb/in
@Temperature -40.0 °F
Practical Use (Water Absorption 1.8%); ASTM-D256
 0.700 J/cm
@Temperature 23.0 °C
1.31 ft-lb/in
@Temperature 73.4 °F
Practical Use (Water Absorption 1.8%); ASTM-D256
Taber Abrasion, mg/1000 Cycles 3232CS-17, Absolute Drying; ASTM-D1044
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.00e+8 - 1.00e+9 ohm-cm1.00e+8 - 1.00e+9 ohm-cmPractical Use (Water Absorption 1.8%); ASTM-D257
 1.00e+12 ohm-cm1.00e+12 ohm-cmAbsolute Drying; ASTM-D257
Dielectric Strength  20.0 kV/mm
@Thickness 2.00 mm
508 kV/in
@Thickness 0.0787 in
Practical Use (Water Absorption 1.8%); ASTM-D149
 29.0 kV/mm
@Thickness 2.00 mm
737 kV/in
@Thickness 0.0787 in
Absolute Drying; ASTM-D149
Arc Resistance 15 sec15 secPractical Use (Water Absorption 1.8%); ASTM-D495
 25 sec25 secAbsolute Drying; ASTM-D495
Comparative Tracking Index 350 V350 VIEC Method
 
Thermal PropertiesMetricEnglishComments
CTE, linear 42.0 µm/m-°C23.3 µin/in-°FAbsolute Drying; ASTM-D696
Deflection Temperature at 0.46 MPa (66 psi) 205 °C401 °FAbsolute Drying; ASTM-D648
Deflection Temperature at 1.8 MPa (264 psi) 160 °C320 °FAbsolute Drying; ASTM-D648
Flammability, UL94 V-0V-0
 
Processing PropertiesMetricEnglishComments
Melt Temperature 250 - 285 °C482 - 545 °F
Mold Temperature 60.0 °C140 °F
Injection Pressure 40.0 - 60.0 MPa5800 - 8700 psi

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Toyobo GLAMIDE® T-402FR Nylon-6
Toyobo GLAMIDE® T-808-02 Nylon-6
Toyobo GLAMIDE® T-521 Nylon-6
Toyobo GLAMIDE® TY-791GT 6T-Nylon
Toyobo GLAMIDE® T-402 Nylon-6

PTOY943 / 107494

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.