MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Aluminum 7050-T73651 plate
Categories: Metal; Nonferrous Metal; Aluminum Alloy; 7000 Series Aluminum Alloy

Material Notes: 7050 has very high strength coupled with high resistance to exfoliation corrosion and stress-corrosion cracking, high fracture toughness, and fatigue resistance. This leads to applications in aircraft structures.

Data points with the AA note have been provided by the Aluminum Association, Inc. and are NOT FOR DESIGN.

Composition Notes:
Composition information provided by the Aluminum Association and is not for design.

Key Words: AA7050-T73651; AA7070-T73651, UNS A97050; ISO AlZn6CuMgZr; Aluminium 7050-T73651; Aluminium 7070-T73651; Al7070-T73651
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 2.83 g/cc0.102 lb/in³AA; Typical
 
Mechanical PropertiesMetricEnglishComments
Hardness, Brinell 140140500 kg load with 10 mm ball. Calculated value.
Hardness, Knoop 177177Converted from Brinell Hardness Value
Hardness, Rockwell A 51.651.6Converted from Brinell Hardness Value
Hardness, Rockwell B 8484Converted from Brinell Hardness Value
Hardness, Vickers 162162Converted from Brinell Hardness Value
Tensile Strength, Ultimate 510 MPa
@Temperature 24.0 °C
74000 psi
@Temperature 75.2 °F
T73651 plate
 117 MPa
@Temperature 204 °C,
Time 3.60e+7 sec
17000 psi
@Temperature 399 °F,
Time 10000 hour
T73651 plate
 131 MPa
@Temperature 204 °C,
Time 3.60e+6 sec
19000 psi
@Temperature 399 °F,
Time 1000 hour
T73651 plate
 159 MPa
@Temperature 177 °C,
Time 3.60e+7 sec
23100 psi
@Temperature 351 °F,
Time 10000 hour
T73651 plate
 165 MPa
@Temperature 204 °C,
Time 360000 sec
23900 psi
@Temperature 399 °F,
Time 100 hour
T73651 plate
 193 MPa
@Temperature 177 °C,
Time 3.60e+6 sec
28000 psi
@Temperature 351 °F,
Time 1000 hour
T73651 plate
 221 MPa
@Temperature 149 °C,
Time 3.60e+7 sec
32100 psi
@Temperature 300 °F,
Time 10000 hour
T73651 plate
 221 MPa
@Temperature 204 °C,
Time 36000 sec
32100 psi
@Temperature 399 °F,
Time 10.0 hour
T73651 plate
 248 MPa
@Temperature 177 °C,
Time 360000 sec
36000 psi
@Temperature 351 °F,
Time 100 hour
T73651 plate
 290 MPa
@Temperature 149 °C,
Time 3.60e+6 sec
42100 psi
@Temperature 300 °F,
Time 1000 hour
T73651 plate
 290 MPa
@Temperature 204 °C,
Time 1800 sec
42100 psi
@Temperature 399 °F,
Time 0.500 hour
T73651 plate
 303 MPa
@Temperature 204 °C,
Time 360 sec
43900 psi
@Temperature 399 °F,
Time 0.100 hour
T73651 plate
 324 MPa
@Temperature 177 °C,
Time 36000 sec
47000 psi
@Temperature 351 °F,
Time 10.0 hour
T73651 plate
 352 MPa
@Temperature 177 °C,
Time 1800 sec
51100 psi
@Temperature 351 °F,
Time 0.500 hour
T73651 plate
 359 MPa
@Temperature 149 °C,
Time 360000 sec
52100 psi
@Temperature 300 °F,
Time 100 hour
T73651 plate
 359 MPa
@Temperature 177 °C,
Time 360 sec
52100 psi
@Temperature 351 °F,
Time 0.100 hour
T73651 plate
 393 MPa
@Temperature 149 °C,
Time 1800 sec
57000 psi
@Temperature 300 °F,
Time 0.500 hour
T73651 plate
 393 MPa
@Temperature 149 °C,
Time 36000 sec
57000 psi
@Temperature 300 °F,
Time 10.0 hour
T73651 plate
 393 MPa
@Temperature 149 °C,
Time 360 sec
57000 psi
@Temperature 300 °F,
Time 0.100 hour
T73651 plate
 441 MPa
@Temperature 100 °C,
Time 360 - 36000 sec
64000 psi
@Temperature 212 °F,
Time 0.100 - 10.0 hour
T73651 plate
 441 MPa
@Temperature 100 °C,
Time 3.60e+6 sec
64000 psi
@Temperature 212 °F,
Time 1000 hour
T73651 plate
 441 MPa
@Temperature 100 °C,
Time 3.60e+7 sec
64000 psi
@Temperature 212 °F,
Time 10000 hour
T73651 plate
 448 MPa
@Temperature 100 °C,
Time 360000 sec
65000 psi
@Temperature 212 °F,
Time 100 hour
T73651 plate
 510 MPa
@Treatment Temp. 24.0 °C
74000 psi
@Treatment Temp. 75.2 °F
T73651 plate
 234 MPa
@Treatment Temp. 204 °C,
Time 3.60e+7 sec
33900 psi
@Treatment Temp. 399 °F,
Time 10000 hour
T73651 plate
 248 MPa
@Treatment Temp. 177 °C,
Time 3.60e+7 sec
36000 psi
@Treatment Temp. 351 °F,
Time 10000 hour
T73651 plate
 262 MPa
@Treatment Temp. 204 °C,
Time 3.60e+6 sec
38000 psi
@Treatment Temp. 399 °F,
Time 1000 hour
T73651 plate
 317 MPa
@Treatment Temp. 177 °C,
Time 3.60e+6 sec
46000 psi
@Treatment Temp. 351 °F,
Time 1000 hour
T73651 plate
 317 MPa
@Treatment Temp. 204 °C,
Time 360000 sec
46000 psi
@Treatment Temp. 399 °F,
Time 100 hour
T73651 plate
 331 MPa
@Treatment Temp. 149 °C,
Time 3.60e+7 sec
48000 psi
@Treatment Temp. 300 °F,
Time 10000 hour
T73651 plate
 386 MPa
@Treatment Temp. 177 °C,
Time 360000 sec
56000 psi
@Treatment Temp. 351 °F,
Time 100 hour
T73651 plate
 386 MPa
@Treatment Temp. 204 °C,
Time 36000 sec
56000 psi
@Treatment Temp. 399 °F,
Time 10.0 hour
T73651 plate
 407 MPa
@Treatment Temp. 149 °C,
Time 3.60e+6 sec
59000 psi
@Treatment Temp. 300 °F,
Time 1000 hour
T73651 plate
 469 MPa
@Treatment Temp. 177 °C,
Time 36000 sec
68000 psi
@Treatment Temp. 351 °F,
Time 10.0 hour
T73651 plate
 469 MPa
@Treatment Temp. 204 °C,
Time 1800 sec
68000 psi
@Treatment Temp. 399 °F,
Time 0.500 hour
T73651 plate
 483 MPa
@Treatment Temp. 149 °C,
Time 360000 sec
70100 psi
@Treatment Temp. 300 °F,
Time 100 hour
T73651 plate
 490 MPa
@Treatment Temp. 204 °C,
Time 360 sec
71100 psi
@Treatment Temp. 399 °F,
Time 0.100 hour
T73651 plate
 496 MPa
@Treatment Temp. 177 °C,
Time 1800 sec
71900 psi
@Treatment Temp. 351 °F,
Time 0.500 hour
T73651 plate
 503 MPa
@Treatment Temp. 149 °C,
Time 36000 sec
73000 psi
@Treatment Temp. 300 °F,
Time 10.0 hour
T73651 plate
 510 MPa
@Treatment Temp. 100 °C,
Time 3.60e+7 sec
74000 psi
@Treatment Temp. 212 °F,
Time 10000 hour
T73651 plate
 510 MPa
@Treatment Temp. 149 °C,
Time 360 sec
74000 psi
@Treatment Temp. 300 °F,
Time 0.100 hour
T73651 plate
 510 MPa
@Treatment Temp. 149 °C,
Time 1800 sec
74000 psi
@Treatment Temp. 300 °F,
Time 0.500 hour
T73651 plate
 510 MPa
@Treatment Temp. 177 °C,
Time 360 sec
74000 psi
@Treatment Temp. 351 °F,
Time 0.100 hour
T73651 plate
 510 MPa
@Treatment Temp. 100 °C,
Time 360 - 36000 sec
74000 psi
@Treatment Temp. 212 °F,
Time 0.100 - 10.0 hour
T73651 plate
 510 MPa
@Treatment Temp. 100 °C,
Time 360000 sec
74000 psi
@Treatment Temp. 212 °F,
Time 100 hour
T73651 plate
 510 MPa
@Treatment Temp. 100 °C,
Time 3.60e+6 sec
74000 psi
@Treatment Temp. 212 °F,
Time 1000 hour
T73651 plate
Tensile Strength, Yield 455 MPa
@Temperature 24.0 °C
66000 psi
@Temperature 75.2 °F
T73651 plate
 90.0 MPa
@Temperature 204 °C,
Time 3.60e+7 sec
13100 psi
@Temperature 399 °F,
Time 10000 hour
T73651 plate
 110 MPa
@Temperature 204 °C,
Time 3.60e+6 sec
16000 psi
@Temperature 399 °F,
Time 1000 hour
T73651 plate
 124 MPa
@Temperature 177 °C,
Time 3.60e+7 sec
18000 psi
@Temperature 351 °F,
Time 10000 hour
T73651 plate
 152 MPa
@Temperature 204 °C,
Time 360000 sec
22000 psi
@Temperature 399 °F,
Time 100 hour
T73651 plate
 172 MPa
@Temperature 177 °C,
Time 3.60e+6 sec
24900 psi
@Temperature 351 °F,
Time 1000 hour
T73651 plate
 193 MPa
@Temperature 149 °C,
Time 3.60e+7 sec
28000 psi
@Temperature 300 °F,
Time 10000 hour
T73651 plate
 207 MPa
@Temperature 204 °C,
Time 36000 sec
30000 psi
@Temperature 399 °F,
Time 10.0 hour
T73651 plate
 234 MPa
@Temperature 177 °C,
Time 360000 sec
33900 psi
@Temperature 351 °F,
Time 100 hour
T73651 plate
 276 MPa
@Temperature 149 °C,
Time 3.60e+6 sec
40000 psi
@Temperature 300 °F,
Time 1000 hour
T73651 plate
 276 MPa
@Temperature 204 °C,
Time 1800 sec
40000 psi
@Temperature 399 °F,
Time 0.500 hour
T73651 plate
 290 MPa
@Temperature 204 °C,
Time 360 sec
42100 psi
@Temperature 399 °F,
Time 0.100 hour
T73651 plate
 310 MPa
@Temperature 177 °C,
Time 36000 sec
45000 psi
@Temperature 351 °F,
Time 10.0 hour
T73651 plate
 332 MPa
@Temperature 149 °C,
Time 360000 sec
48200 psi
@Temperature 300 °F,
Time 100 hour
T73651 plate
 345 MPa
@Temperature 177 °C,
Time 360 sec
50000 psi
@Temperature 351 °F,
Time 0.100 hour
T73651 plate
 345 MPa
@Temperature 177 °C,
Time 1800 sec
50000 psi
@Temperature 351 °F,
Time 0.500 hour
T73651 plate
 386 MPa
@Temperature 149 °C,
Time 360 sec
56000 psi
@Temperature 300 °F,
Time 0.100 hour
T73651 plate
 386 MPa
@Temperature 149 °C,
Time 1800 sec
56000 psi
@Temperature 300 °F,
Time 0.500 hour
T73651 plate
 386 MPa
@Temperature 149 °C,
Time 36000 sec
56000 psi
@Temperature 300 °F,
Time 10.0 hour
T73651 plate
 421 MPa
@Temperature 100 °C,
Time 3.60e+7 sec
61100 psi
@Temperature 212 °F,
Time 10000 hour
T73651 plate
 427 MPa
@Temperature 100 °C,
Time 360 - 36000 sec
61900 psi
@Temperature 212 °F,
Time 0.100 - 10.0 hour
T73651 plate
 427 MPa
@Temperature 100 °C,
Time 3.60e+6 sec
61900 psi
@Temperature 212 °F,
Time 1000 hour
T73651 plate
 434 MPa
@Temperature 100 °C,
Time 360000 sec
62900 psi
@Temperature 212 °F,
Time 100 hour
T73651 plate
 455 MPa
@Treatment Temp. 24.0 °C
66000 psi
@Treatment Temp. 75.2 °F
T73651 plate
 117 MPa
@Treatment Temp. 204 °C,
Time 3.60e+7 sec
17000 psi
@Treatment Temp. 399 °F,
Time 10000 hour
T73651 plate
 138 MPa
@Treatment Temp. 204 °C,
Time 3.60e+6 sec
20000 psi
@Treatment Temp. 399 °F,
Time 1000 hour
T73651 plate
 152 MPa
@Treatment Temp. 177 °C,
Time 3.60e+7 sec
22000 psi
@Treatment Temp. 351 °F,
Time 10000 hour
T73651 plate
 200 MPa
@Treatment Temp. 204 °C,
Time 360000 sec
29000 psi
@Treatment Temp. 399 °F,
Time 100 hour
T73651 plate
 214 MPa
@Treatment Temp. 177 °C,
Time 3.60e+6 sec
31000 psi
@Treatment Temp. 351 °F,
Time 1000 hour
T73651 plate
 228 MPa
@Treatment Temp. 149 °C,
Time 3.60e+7 sec
33100 psi
@Treatment Temp. 300 °F,
Time 10000 hour
T73651 plate
 283 MPa
@Treatment Temp. 204 °C,
Time 36000 sec
41000 psi
@Treatment Temp. 399 °F,
Time 10.0 hour
T73651 plate
 296 MPa
@Treatment Temp. 177 °C,
Time 360000 sec
42900 psi
@Treatment Temp. 351 °F,
Time 100 hour
T73651 plate
 317 MPa
@Treatment Temp. 149 °C,
Time 3.60e+6 sec
46000 psi
@Treatment Temp. 300 °F,
Time 1000 hour
T73651 plate
 400 MPa
@Treatment Temp. 177 °C,
Time 36000 sec
58000 psi
@Treatment Temp. 351 °F,
Time 10.0 hour
T73651 plate
 407 MPa
@Treatment Temp. 149 °C,
Time 360000 sec
59000 psi
@Treatment Temp. 300 °F,
Time 100 hour
T73651 plate
 421 MPa
@Treatment Temp. 204 °C,
Time 1800 sec
61100 psi
@Treatment Temp. 399 °F,
Time 0.500 hour
T73651 plate
 434 MPa
@Treatment Temp. 204 °C,
Time 360 sec
62900 psi
@Treatment Temp. 399 °F,
Time 0.100 hour
T73651 plate
 441 MPa
@Treatment Temp. 100 °C,
Time 3.60e+7 sec
64000 psi
@Treatment Temp. 212 °F,
Time 10000 hour
T73651 plate
 441 MPa
@Treatment Temp. 149 °C,
Time 36000 sec
64000 psi
@Treatment Temp. 300 °F,
Time 10.0 hour
T73651 plate
 441 MPa
@Treatment Temp. 177 °C,
Time 1800 sec
64000 psi
@Treatment Temp. 351 °F,
Time 0.500 hour
T73651 plate
 448 MPa
@Treatment Temp. 149 °C,
Time 1800 sec
65000 psi
@Treatment Temp. 300 °F,
Time 0.500 hour
T73651 plate
 448 MPa
@Treatment Temp. 177 °C,
Time 360 sec
65000 psi
@Treatment Temp. 351 °F,
Time 0.100 hour
T73651 plate
 455 MPa
@Treatment Temp. 100 °C,
Time 360 - 36000 sec
66000 psi
@Treatment Temp. 212 °F,
Time 0.100 - 10.0 hour
T73651 plate
 455 MPa
@Treatment Temp. 100 °C,
Time 3.60e+6 sec
66000 psi
@Treatment Temp. 212 °F,
Time 1000 hour
T73651 plate
 455 MPa
@Treatment Temp. 149 °C,
Time 360 sec
66000 psi
@Treatment Temp. 300 °F,
Time 0.100 hour
T73651 plate
 462 MPa
@Treatment Temp. 100 °C,
Time 360000 sec
67000 psi
@Treatment Temp. 212 °F,
Time 100 hour
T73651 plate
Elongation at Break 11 %
@Temperature 24.0 °C
11 %
@Temperature 75.2 °F
T73651 plate
 13 %
@Temperature 100 °C,
Time 360 - 36000 sec
13 %
@Temperature 212 °F,
Time 0.100 - 10.0 hour
T73651 plate
 13 %
@Temperature 100 °C,
Time 360000 sec
13 %
@Temperature 212 °F,
Time 100 hour
T73651 plate
 14 %
@Temperature 100 °C,
Time 3.60e+6 sec
14 %
@Temperature 212 °F,
Time 1000 hour
T73651 plate
 15 %
@Temperature 100 °C,
Time 3.60e+7 sec
15 %
@Temperature 212 °F,
Time 10000 hour
T73651 plate
 16 %
@Temperature 149 °C,
Time 360 sec
16 %
@Temperature 300 °F,
Time 0.100 hour
T73651 plate
 17 %
@Temperature 149 °C,
Time 1800 sec
17 %
@Temperature 300 °F,
Time 0.500 hour
T73651 plate
 18 %
@Temperature 149 °C,
Time 36000 sec
18 %
@Temperature 300 °F,
Time 10.0 hour
T73651 plate
 19 %
@Temperature 149 °C,
Time 360000 sec
19 %
@Temperature 300 °F,
Time 100 hour
T73651 plate
 19 %
@Temperature 177 °C,
Time 360 sec
19 %
@Temperature 351 °F,
Time 0.100 hour
T73651 plate
 20 %
@Temperature 177 °C,
Time 1800 sec
20 %
@Temperature 351 °F,
Time 0.500 hour
T73651 plate
 21 %
@Temperature 149 °C,
Time 3.60e+6 sec
21 %
@Temperature 300 °F,
Time 1000 hour
T73651 plate
 22 %
@Temperature 177 °C,
Time 36000 sec
22 %
@Temperature 351 °F,
Time 10.0 hour
T73651 plate
 22 %
@Temperature 204 °C,
Time 360 sec
22 %
@Temperature 399 °F,
Time 0.100 hour
T73651 plate
 23 %
@Temperature 204 °C,
Time 1800 sec
23 %
@Temperature 399 °F,
Time 0.500 hour
T73651 plate
 25 %
@Temperature 177 °C,
Time 360000 sec
25 %
@Temperature 351 °F,
Time 100 hour
T73651 plate
 27 %
@Temperature 204 °C,
Time 36000 sec
27 %
@Temperature 399 °F,
Time 10.0 hour
T73651 plate
 29 %
@Temperature 149 °C,
Time 3.60e+7 sec
29 %
@Temperature 300 °F,
Time 10000 hour
T73651 plate
 31 %
@Temperature 177 °C,
Time 3.60e+6 sec
31 %
@Temperature 351 °F,
Time 1000 hour
T73651 plate
 32 %
@Temperature 204 °C,
Time 360000 sec
32 %
@Temperature 399 °F,
Time 100 hour
T73651 plate
 40 %
@Temperature 177 °C,
Time 3.60e+7 sec
40 %
@Temperature 351 °F,
Time 10000 hour
T73651 plate
 45 %
@Temperature 204 °C,
Time 3.60e+6 sec
45 %
@Temperature 399 °F,
Time 1000 hour
T73651 plate
 54 %
@Temperature 204 °C,
Time 3.60e+7 sec
54 %
@Temperature 399 °F,
Time 10000 hour
T73651 plate
 11 %
@Treatment Temp. 24.0 °C
11 %
@Treatment Temp. 75.2 °F
T73651 plate
 11 %
@Treatment Temp. 100 °C,
Time 360 - 36000 sec
11 %
@Treatment Temp. 212 °F,
Time 0.100 - 10.0 hour
T73651 plate
 11 %
@Treatment Temp. 149 °C,
Time 360 sec
11 %
@Treatment Temp. 300 °F,
Time 0.100 hour
T73651 plate
 12 %
@Treatment Temp. 100 °C,
Time 360000 sec
12 %
@Treatment Temp. 212 °F,
Time 100 hour
T73651 plate
 12 %
@Treatment Temp. 100 °C,
Time 3.60e+6 sec
12 %
@Treatment Temp. 212 °F,
Time 1000 hour
T73651 plate
 12 %
@Treatment Temp. 100 °C,
Time 3.60e+7 sec
12 %
@Treatment Temp. 212 °F,
Time 10000 hour
T73651 plate
 12 %
@Treatment Temp. 149 °C,
Time 1800 sec
12 %
@Treatment Temp. 300 °F,
Time 0.500 hour
T73651 plate
 12 %
@Treatment Temp. 149 °C,
Time 36000 sec
12 %
@Treatment Temp. 300 °F,
Time 10.0 hour
T73651 plate
 12 %
@Treatment Temp. 177 °C,
Time 360 sec
12 %
@Treatment Temp. 351 °F,
Time 0.100 hour
T73651 plate
 12 %
@Treatment Temp. 177 °C,
Time 1800 sec
12 %
@Treatment Temp. 351 °F,
Time 0.500 hour
T73651 plate
 12 %
@Treatment Temp. 204 °C,
Time 360 sec
12 %
@Treatment Temp. 399 °F,
Time 0.100 hour
T73651 plate
 12 %
@Treatment Temp. 204 °C,
Time 1800 sec
12 %
@Treatment Temp. 399 °F,
Time 0.500 hour
T73651 plate
 13 %
@Treatment Temp. 149 °C,
Time 360000 sec
13 %
@Treatment Temp. 300 °F,
Time 100 hour
T73651 plate
 13 %
@Treatment Temp. 149 °C,
Time 3.60e+6 sec
13 %
@Treatment Temp. 300 °F,
Time 1000 hour
T73651 plate
 13 %
@Treatment Temp. 177 °C,
Time 36000 sec
13 %
@Treatment Temp. 351 °F,
Time 10.0 hour
T73651 plate
 13 %
@Treatment Temp. 177 °C,
Time 360000 sec
13 %
@Treatment Temp. 351 °F,
Time 100 hour
T73651 plate
 13 %
@Treatment Temp. 204 °C,
Time 36000 sec
13 %
@Treatment Temp. 399 °F,
Time 10.0 hour
T73651 plate
 14 %
@Treatment Temp. 149 °C,
Time 3.60e+7 sec
14 %
@Treatment Temp. 300 °F,
Time 10000 hour
T73651 plate
 14 %
@Treatment Temp. 177 °C,
Time 3.60e+6 sec
14 %
@Treatment Temp. 351 °F,
Time 1000 hour
T73651 plate
 14 %
@Treatment Temp. 204 °C,
Time 360000 sec
14 %
@Treatment Temp. 399 °F,
Time 100 hour
T73651 plate
 15 %
@Treatment Temp. 177 °C,
Time 3.60e+7 sec
15 %
@Treatment Temp. 351 °F,
Time 10000 hour
T73651 plate
 16 %
@Treatment Temp. 204 °C,
Time 3.60e+6 sec
16 %
@Treatment Temp. 399 °F,
Time 1000 hour
T73651 plate
 19 %
@Treatment Temp. 204 °C,
Time 3.60e+7 sec
19 %
@Treatment Temp. 399 °F,
Time 10000 hour
T73651 plate
Creep Strength  124 MPa
@Temperature 149 °C,
Time 3.60e+6 sec
18000 psi
@Temperature 300 °F,
Time 1000 hour
T73651 plate; 0.1% creep
 145 MPa
@Temperature 149 °C,
Time 3.60e+6 sec
21000 psi
@Temperature 300 °F,
Time 1000 hour
T73651 plate; 0.2% creep
 152 MPa
@Temperature 149 °C,
Time 360000 sec
22000 psi
@Temperature 300 °F,
Time 100 hour
T73651 plate; 0.1% creep
 165 MPa
@Temperature 149 °C,
Time 3.60e+6 sec
23900 psi
@Temperature 300 °F,
Time 1000 hour
T73651 plate; 0.5% creep
 179 MPa
@Temperature 149 °C,
Time 3.60e+6 sec
26000 psi
@Temperature 300 °F,
Time 1000 hour
T73651 plate; 1.0% creep
 193 MPa
@Temperature 149 °C,
Time 360000 sec
28000 psi
@Temperature 300 °F,
Time 100 hour
T73651 plate; 0.2% creep
 228 MPa
@Temperature 149 °C,
Time 36000 sec
33100 psi
@Temperature 300 °F,
Time 10.0 hour
T73651 plate; 0.1% creep
 241 MPa
@Temperature 149 °C,
Time 360000 sec
35000 psi
@Temperature 300 °F,
Time 100 hour
T73651 plate; 0.5% creep
 255 MPa
@Temperature 149 °C,
Time 360000 sec
37000 psi
@Temperature 300 °F,
Time 100 hour
T73651 plate; 1.0% creep
 269 MPa
@Temperature 149 °C,
Time 36000 sec
39000 psi
@Temperature 300 °F,
Time 10.0 hour
T73651 plate; 0.2% creep
 290 MPa
@Temperature 149 °C,
Time 36000 sec
42100 psi
@Temperature 300 °F,
Time 10.0 hour
T73651 plate; 0.5% creep
 290 MPa
@Temperature 149 °C,
Time 3600 sec
42100 psi
@Temperature 300 °F,
Time 1.00 hour
T73651 plate; 0.1% creep
 303 MPa
@Temperature 149 °C,
Time 36000 sec
43900 psi
@Temperature 300 °F,
Time 10.0 hour
T73651 plate; 1.0% creep
 303 MPa
@Temperature 149 °C,
Time 3600 sec
43900 psi
@Temperature 300 °F,
Time 1.00 hour
T73651 plate; 0.2% creep
 317 MPa
@Temperature 100 °C,
Time 3.60e+6 sec
46000 psi
@Temperature 212 °F,
Time 1000 hour
T73651 plate; 0.2% creep
 324 MPa
@Temperature 149 °C,
Time 3600 sec
47000 psi
@Temperature 300 °F,
Time 1.00 hour
T73651 plate; 0.5% creep
 324 MPa
@Temperature 149 °C,
Time 360 sec
47000 psi
@Temperature 300 °F,
Time 0.100 hour
T73651 plate; 0.1% creep
 331 MPa
@Temperature 100 °C,
Time 360000 sec
48000 psi
@Temperature 212 °F,
Time 100 hour
T73651 plate; 0.1% creep
 338 MPa
@Temperature 149 °C,
Time 3600 sec
49000 psi
@Temperature 300 °F,
Time 1.00 hour
T73651 plate; 1.0% creep
 345 MPa
@Temperature 100 °C,
Time 3.60e+6 sec
50000 psi
@Temperature 212 °F,
Time 1000 hour
T73651 plate; 0.5% creep
 345 MPa
@Temperature 100 °C,
Time 360000 sec
50000 psi
@Temperature 212 °F,
Time 100 hour
T73651 plate; 0.2% creep
 345 MPa
@Temperature 149 °C,
Time 360 sec
50000 psi
@Temperature 300 °F,
Time 0.100 hour
T73651 plate; 0.2% creep
 352 MPa
@Temperature 100 °C,
Time 3.60e+6 sec
51100 psi
@Temperature 212 °F,
Time 1000 hour
T73651 plate; 1.0% creep
 359 MPa
@Temperature 149 °C,
Time 360 sec
52100 psi
@Temperature 300 °F,
Time 0.100 hour
T73651 plate; 0.5% creep
 359 MPa
@Temperature 100 °C,
Time 36000 sec
52100 psi
@Temperature 212 °F,
Time 10.0 hour
T73651 plate; 0.1% creep
 365 MPa
@Temperature 149 °C,
Time 360 sec
52900 psi
@Temperature 300 °F,
Time 0.100 hour
T73651 plate; 1.0% creep
 365 MPa
@Temperature 100 °C,
Time 360000 sec
52900 psi
@Temperature 212 °F,
Time 100 hour
T73651 plate; 0.5% creep
 372 MPa
@Temperature 100 °C,
Time 360000 sec
54000 psi
@Temperature 212 °F,
Time 100 hour
T73651 plate; 1.0% creep
 372 MPa
@Temperature 100 °C,
Time 36000 sec
54000 psi
@Temperature 212 °F,
Time 10.0 hour
T73651 plate; 0.2% creep
 386 MPa
@Temperature 100 °C,
Time 36000 sec
56000 psi
@Temperature 212 °F,
Time 10.0 hour
T73651 plate; 0.5% creep
 386 MPa
@Temperature 100 °C,
Time 3600 sec
56000 psi
@Temperature 212 °F,
Time 1.00 hour
T73651 plate; 0.1% creep
 393 MPa
@Temperature 100 °C,
Time 36000 sec
57000 psi
@Temperature 212 °F,
Time 10.0 hour
T73651 plate; 1.0% creep
 400 MPa
@Temperature 100 °C,
Time 3600 sec
58000 psi
@Temperature 212 °F,
Time 1.00 hour
T73651 plate; 0.2% creep
 407 MPa
@Temperature 100 °C,
Time 3600 sec
59000 psi
@Temperature 212 °F,
Time 1.00 hour
T73651 plate; 0.5% creep
 414 MPa
@Temperature 100 °C,
Time 3600 sec
60000 psi
@Temperature 212 °F,
Time 1.00 hour
T73651 plate; 1.0% creep
 414 MPa
@Temperature 100 °C,
Time 360 sec
60000 psi
@Temperature 212 °F,
Time 0.100 hour
T73651 plate; 0.1% creep
 421 MPa
@Temperature 100 °C,
Time 360 sec
61100 psi
@Temperature 212 °F,
Time 0.100 hour
T73651 plate; 0.2% creep
 427 MPa
@Temperature 100 °C,
Time 360 sec
61900 psi
@Temperature 212 °F,
Time 0.100 hour
T73651 plate; 0.5% creep
 434 MPa
@Temperature 100 °C,
Time 360 sec
62900 psi
@Temperature 212 °F,
Time 0.100 hour
T73651 plate; 1.0% creep
 434 MPa
@Temperature 24.0 °C,
Time 360000 sec
62900 psi
@Temperature 75.2 °F,
Time 100 hour
T73651 plate; 0.1% creep
 441 MPa
@Temperature 24.0 °C,
Time 3.60e+6 sec
64000 psi
@Temperature 75.2 °F,
Time 1000 hour
T73651 plate; 0.5% creep
 441 MPa
@Temperature 24.0 °C,
Time 36000 sec
64000 psi
@Temperature 75.2 °F,
Time 10.0 hour
T73651 plate; 0.2% creep
 441 MPa
@Temperature 24.0 °C,
Time 360000 sec
64000 psi
@Temperature 75.2 °F,
Time 100 hour
T73651 plate; 0.2% creep
 441 MPa
@Temperature 24.0 °C,
Time 3600 sec
64000 psi
@Temperature 75.2 °F,
Time 1.00 hour
T73651 plate; 0.1% creep
 441 MPa
@Temperature 24.0 °C,
Time 36000 sec
64000 psi
@Temperature 75.2 °F,
Time 10.0 hour
T73651 plate; 0.1% creep
 448 MPa
@Temperature 24.0 °C,
Time 3.60e+6 sec
65000 psi
@Temperature 75.2 °F,
Time 1000 hour
T73651 plate; 1.0% creep
 448 MPa
@Temperature 24.0 °C,
Time 360000 sec
65000 psi
@Temperature 75.2 °F,
Time 100 hour
T73651 plate; 0.5% creep
 448 MPa
@Temperature 24.0 °C,
Time 3600 sec
65000 psi
@Temperature 75.2 °F,
Time 1.00 hour
T73651 plate; 0.2% creep
 448 MPa
@Temperature 24.0 °C,
Time 360 sec
65000 psi
@Temperature 75.2 °F,
Time 0.100 hour
T73651 plate; 0.1% creep
 455 MPa
@Temperature 24.0 °C,
Time 360000 sec
66000 psi
@Temperature 75.2 °F,
Time 100 hour
T73651 plate; 1.0% creep
 455 MPa
@Temperature 24.0 °C,
Time 36000 sec
66000 psi
@Temperature 75.2 °F,
Time 10.0 hour
T73651 plate; 0.5% creep
 455 MPa
@Temperature 24.0 °C,
Time 360 sec
66000 psi
@Temperature 75.2 °F,
Time 0.100 hour
T73651 plate; 0.2% creep
 462 MPa
@Temperature 24.0 °C,
Time 3600 sec
67000 psi
@Temperature 75.2 °F,
Time 1.00 hour
T73651 plate; 0.5% creep
 469 MPa
@Temperature 24.0 °C,
Time 36000 sec
68000 psi
@Temperature 75.2 °F,
Time 10.0 hour
T73651 plate; 1.0% creep
 476 MPa
@Temperature 24.0 °C,
Time 360 sec
69000 psi
@Temperature 75.2 °F,
Time 0.100 hour
T73651 plate; 0.5% creep
 483 MPa
@Temperature 24.0 °C,
Time 3600 sec
70100 psi
@Temperature 75.2 °F,
Time 1.00 hour
T73651 plate; 1.0% creep
 496 MPa
@Temperature 24.0 °C,
Time 360 sec
71900 psi
@Temperature 75.2 °F,
Time 0.100 hour
T73651 plate; 1.0% creep
Rupture Strength  179 MPa
@Temperature 149 °C,
Time 3.60e+6 sec
26000 psi
@Temperature 300 °F,
Time 1000 hour
T73651 plate
 262 MPa
@Temperature 149 °C,
Time 360000 sec
38000 psi
@Temperature 300 °F,
Time 100 hour
T73651 plate
 310 MPa
@Temperature 149 °C,
Time 36000 sec
45000 psi
@Temperature 300 °F,
Time 10.0 hour
T73651 plate
 345 MPa
@Temperature 149 °C,
Time 3600 sec
50000 psi
@Temperature 300 °F,
Time 1.00 hour
T73651 plate
 359 MPa
@Temperature 100 °C,
Time 3.60e+6 sec
52100 psi
@Temperature 212 °F,
Time 1000 hour
T73651 plate
 372 MPa
@Temperature 149 °C,
Time 360 sec
54000 psi
@Temperature 300 °F,
Time 0.100 hour
T73651 plate
 379 MPa
@Temperature 100 °C,
Time 360000 sec
55000 psi
@Temperature 212 °F,
Time 100 hour
T73651 plate
 407 MPa
@Temperature 100 °C,
Time 36000 sec
59000 psi
@Temperature 212 °F,
Time 10.0 hour
T73651 plate
 427 MPa
@Temperature 100 °C,
Time 3600 sec
61900 psi
@Temperature 212 °F,
Time 1.00 hour
T73651 plate
 441 MPa
@Temperature 100 °C,
Time 360 sec
64000 psi
@Temperature 212 °F,
Time 0.100 hour
T73651 plate
 469 MPa
@Temperature 24.0 °C,
Time 3.60e+6 sec
68000 psi
@Temperature 75.2 °F,
Time 1000 hour
T73651 plate
 476 MPa
@Temperature 24.0 °C,
Time 360000 sec
69000 psi
@Temperature 75.2 °F,
Time 100 hour
T73651 plate
 490 MPa
@Temperature 24.0 °C,
Time 36000 sec
71100 psi
@Temperature 75.2 °F,
Time 10.0 hour
T73651 plate
 503 MPa
@Temperature 24.0 °C,
Time 3600 sec
73000 psi
@Temperature 75.2 °F,
Time 1.00 hour
T73651 plate
 510 MPa
@Temperature 24.0 °C,
Time 360 sec
74000 psi
@Temperature 75.2 °F,
Time 0.100 hour
T73651 plate
Modulus of Elasticity 71.7 GPa10400 ksiAA; Typical; Average of tension and compression. Compression modulus is about 2% greater than tensile modulus.
Poissons Ratio 0.330.33
Fracture Toughness >= 22.0 MPa-m½>= 20.0 ksi-in½S-L, Plane-strain
 >= 24.2 MPa-m½>= 22.0 ksi-in½T-L, Plane-strain
 >= 26.4 MPa-m½>= 24.0 ksi-in½L-T, Plane-strain
 28.6 MPa-m½26.0 ksi-in½average; S-L, Plane-strain
 29.7 MPa-m½27.0 ksi-in½average; T-L, Plane-strain
 35.2 MPa-m½32.0 ksi-in½average; L-T, Plane-strain
Shear Modulus 26.9 GPa3900 ksi
Shear Strength 303 MPa44000 psiAA; Typical
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.00000430 ohm-cm0.00000430 ohm-cm
 
Thermal PropertiesMetricEnglishComments
CTE, linear  21.7 µm/m-°C
@Temperature -50.0 - 20.0 °C
12.1 µin/in-°F
@Temperature -58.0 - 68.0 °F
 23.0 µm/m-°C
@Temperature 20.0 - 100 °C
12.8 µin/in-°F
@Temperature 68.0 - 212 °F
AA; Typical; average over range
 23.5 µm/m-°C
@Temperature 20.0 - 100 °C
13.1 µin/in-°F
@Temperature 68.0 - 212 °F
 24.4 µm/m-°C
@Temperature 20.0 - 200 °C
13.6 µin/in-°F
@Temperature 68.0 - 392 °F
 25.4 µm/m-°C
@Temperature 20.0 - 300 °C
14.1 µin/in-°F
@Temperature 68.0 - 572 °F
Specific Heat Capacity 0.860 J/g-°C0.206 BTU/lb-°F
Thermal Conductivity 157 W/m-K1090 BTU-in/hr-ft²-°F
Melting Point 488 - 629.4 °C910 - 1165 °FAA; Typical range based on typical composition for wrought products >= 1/4 in. thickness
Solidus 488 °C910 °FAA; Typical
Liquidus 629.4 °C1165 °FAA; Typical
 
Processing PropertiesMetricEnglishComments
Annealing Temperature 413 °C775 °F
Solution Temperature 477 °C890 °F
Aging Temperature 121 - 177 °C250 - 350 °F
 
Component Elements PropertiesMetricEnglishComments
Aluminum, Al 87.3 - 90.3 %87.3 - 90.3 %As remainder
Chromium, Cr <= 0.04 %<= 0.04 %
Copper, Cu 2.0 - 2.6 %2.0 - 2.6 %
Iron, Fe <= 0.15 %<= 0.15 %
Magnesium, Mg 1.9 - 2.6 %1.9 - 2.6 %
Manganese, Mn <= 0.10 %<= 0.10 %
Other, each <= 0.05 %<= 0.05 %
Other, total <= 0.15 %<= 0.15 %
Silicon, Si <= 0.12 %<= 0.12 %
Titanium, Ti <= 0.06 %<= 0.06 %
Zinc, Zn 5.7 - 6.7 %5.7 - 6.7 %
Zirconium, Zr 0.08 - 0.15 %0.08 - 0.15 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Aluminum 7050-T73511; 7050-T73510
Aluminum 7050-T73652 forgings
Aluminum 7050-T74
Aluminum 7050-T7651
Aluminum 7050-T7451 (7050-T73651)

MA7050T73a / 156323

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.