MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Metalmen Sales

Aluminum 7050-T73511; 7050-T73510
Categories: Metal; Nonferrous Metal; Aluminum Alloy; 7000 Series Aluminum Alloy

Material Notes: 7050 has very high strength coupled with high resistance to exfoliation corrosion and stress-corrosion cracking, high fracture toughness, and fatigue resistance. This leads to applications in aircraft structures.

Data points with the AA note have been provided by the Aluminum Association, Inc. and are NOT FOR DESIGN.

Composition Notes:
Composition information provided by the Aluminum Association and is not for design.

Key Words: UNS A97050; ISO AlZn6CuMgZr; Aluminum 7050-T73510; AA7050-T73511; Al7050-T73511
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 2.83 g/cc0.102 lb/in³AA; Typical
 
Mechanical PropertiesMetricEnglishComments
Hardness, Brinell 132132500 kg load with 10 mm ball. Calculated value.
Hardness, Knoop 166166Converted from Brinell Hardness Value
Hardness, Rockwell A 49.849.8Converted from Brinell Hardness Value
Hardness, Rockwell B 8080Converted from Brinell Hardness Value
Hardness, Vickers 151151Converted from Brinell Hardness Value
Tensile Strength, Ultimate 496 MPa72000 psiAA; Typical
Tensile Strength, Yield 434 MPa63000 psiAA; Typical
Elongation at Break 12 %
@Diameter 12.7 mm
12 %
@Diameter 0.500 in
AA; Typical
Modulus of Elasticity 71.7 GPa10400 ksiAA; Typical; Average of tension and compression. Compression modulus is about 2% greater than tensile modulus.
Poissons Ratio 0.330.33
Fracture Toughness 26.4 MPa-m½24.0 ksi-in½average; S-L
 31.9 MPa-m½29.0 ksi-in½average; T-L
 45.1 MPa-m½41.0 ksi-in½average; L-T
Shear Modulus 26.9 GPa3900 ksi
Shear Strength 290 MPa42100 psiCalculated value.
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.00000430 ohm-cm0.00000430 ohm-cm
 
Thermal PropertiesMetricEnglishComments
CTE, linear  21.7 µm/m-°C
@Temperature -50.0 - 20.0 °C
12.1 µin/in-°F
@Temperature -58.0 - 68.0 °F
 23.5 µm/m-°C
@Temperature 20.0 - 100 °C
13.1 µin/in-°F
@Temperature 68.0 - 212 °F
 23.6 µm/m-°C
@Temperature 20.0 - 100 °C
13.1 µin/in-°F
@Temperature 68.0 - 212 °F
 24.4 µm/m-°C
@Temperature 20.0 - 200 °C
13.6 µin/in-°F
@Temperature 68.0 - 392 °F
 25.4 µm/m-°C
@Temperature 20.0 - 300 °C
14.1 µin/in-°F
@Temperature 68.0 - 572 °F
Specific Heat Capacity 0.860 J/g-°C0.206 BTU/lb-°F
Thermal Conductivity 155 W/m-K1080 BTU-in/hr-ft²-°FEstimated from other heat treatments.
Melting Point 524 - 635 °C975 - 1180 °FFor homogeneous wrought material. Eutectic for nonhomogeneous wrought or as-cast material that has not been heat treated is 465ºC.
Solidus 524 °C975 °FFor homogeneous wrought material. Eutectic for nonhomogeneous wrought or as-cast material that has not been heat treated is 465ºC.
Liquidus 635 °C1180 °F
 
Processing PropertiesMetricEnglishComments
Annealing Temperature 413 °C775 °F
Solution Temperature 477 °C890 °F
Aging Temperature 121 - 177 °C250 - 350 °F
 
Component Elements PropertiesMetricEnglishComments
Aluminum, Al 87.3 - 90.3 %87.3 - 90.3 %As remainder
Chromium, Cr <= 0.04 %<= 0.04 %
Copper, Cu 2.0 - 2.6 %2.0 - 2.6 %
Iron, Fe <= 0.15 %<= 0.15 %
Magnesium, Mg 1.9 - 2.6 %1.9 - 2.6 %
Manganese, Mn <= 0.10 %<= 0.10 %
Other, each <= 0.05 %<= 0.05 %
Other, total <= 0.15 %<= 0.15 %
Silicon, Si <= 0.12 %<= 0.12 %
Titanium, Ti <= 0.06 %<= 0.06 %
Zinc, Zn 5.7 - 6.7 %5.7 - 6.7 %
Zirconium, Zr 0.08 - 0.15 %0.08 - 0.15 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Aluminum 7050-T73651 plate
Aluminum 7050-T7451 (7050-T73651)
Aluminum 7050-T74
Aluminum 7050-T7651
Aluminum 7050-T73652 forgings

MA7050T735 / 9575

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.