MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Celanese Zenite® 6635 BK010 LCP
Categories: Polymer; Thermoplastic; Liquid Crystal Polymer (LCP); Liquid Crystal Polymer (LCP), Mineral Filled

Material Notes: Zenite® 6635 BK010 is a 40% glass/mineral reinforced liquid crystal polymer resin having excellent flow and weldline strength.

Celenese acquired the Zenite product line from DuPont in 2010.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.74 g/cc0.0629 lb/in³ISO 1183
Filler Content 40 %40 %
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 100 MPa14500 psiISO 527
Elongation at Break 3.2 %3.2 %ISO 527
Tensile Modulus 9.00 GPa1310 ksiISO 527
Flexural Strength 140 MPa
@Temperature 23.0 °C
20300 psi
@Temperature 73.4 °F
ISO 178
Flexural Modulus 7.20 GPa
@Temperature 23.0 °C
1040 ksi
@Temperature 73.4 °F
ISO 178
Charpy Impact, Notched 0.700 J/cm²
@Temperature 23.0 °C
3.33 ft-lb/in²
@Temperature 73.4 °F
ISO 179/1eA
 
Electrical PropertiesMetricEnglishComments
Comparative Tracking Index 175 V175 VIEC 60112
 
Thermal PropertiesMetricEnglishComments
Melting Point 335 °C635 °F10°C/min; ISO 11357-1/-3
Deflection Temperature at 1.8 MPa (264 psi) 240 °C464 °FISO 75-1/-2
UL RTI, Electrical 130 °C
@Thickness 1.50 mm
266 °F
@Thickness 0.0591 in
UL 746B
UL RTI, Mechanical with Impact 130 °C
@Thickness 1.50 mm
266 °F
@Thickness 0.0591 in
UL 746B
UL RTI, Mechanical without Impact 130 °C
@Thickness 1.50 mm
266 °F
@Thickness 0.0591 in
UL 746B
Flammability, UL94  V-0
@Thickness 1.50 mm
V-0
@Thickness 0.0591 in
IEC 60695-11-10
 V-0
@Thickness 1.50 mm
V-0
@Thickness 0.0591 in
UL94
 
Processing PropertiesMetricEnglishComments
Melt Temperature 355 °C671 °FOptimum
 350 - 360 °C662 - 680 °F
Mold Temperature 80.0 °C176 °FOptimum
 40.0 - 150 °C104 - 302 °F
Drying Temperature 150 °C302 °F
Dry Time 3 hour3 hourDehumidified Dryer
Moisture Content <= 0.010 %<= 0.010 %
 
Descriptive Properties
ColorBlack
Drying RecommendedYes
FillerGlass/Mineral
FormsPellets
GenericLCP
Part Marking Code>LCP-(MD+GF)40<ISO 11469
Polymer FamilyLCP
Polymer TypeLCP
Product CategoryElectrical Resins
 Flame Retardant Resins
 Glass/Mineral Reinforced Resins
 Low Warp Resins
Region AvailableAmericas
 Asia/Pacific
 Europe
Resin IdentificationLCP-(MD+GF)40ISO 1043

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Celanese ZENITE 7755 LCP, 55% Mineral / Glass Reinforced
Celanese ZENITE 6244L LCP, 40% Mineral / Glass Reinforced
Celanese ZENITE 6130L LCP, 30% Glass Reinforced
Celanese VECTRA E135i LCP, 35% Glass Reinforced
Celanese Zenite® 6330 NC010 LCP (Extended Tabular Temperature Data)

PHCS509 / 89600

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.