MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

AISI Type 316F Stainless Steel, annealed bar
Categories: Metal; Ferrous Metal; Stainless Steel; T 300 Series Stainless Steel

Material Notes: Molybdenum content increases resistance to marine environments. High creep strength at elevated temperatures and good heat resistance. Biocompatible. Fabrication characteristics similar to Types 302 and 304.

Applications: food and pharmaceutical processing equipment, marine exterior trim, surgical implants, and industrial equipment that handles the corrosive process chemicals used to produce inks, rayons, photographic chemicals, paper, textiles, bleaches, and rubber.

Corrosion Resistance: better corrosion resistance than 302 and 304; resists sodium and calcium brines; hypochlorite solutions, phosphoric acid; and the sulfite liquors and sulfurous acids used in the paper pulp industry.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 8.00 g/cc0.289 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Brinell 143143
Hardness, Knoop 163163Converted from Brinell
Hardness, Rockwell B 7878
Hardness, Vickers 149149Converted from Brinell
Tensile Strength, Ultimate 565 MPa81900 psi
Tensile Strength, Yield 240 MPa34800 psi
Elongation at Break 57 %57 %in 50 mm
Modulus of Elasticity 193 GPa28000 ksi
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.0000740 ohm-cm0.0000740 ohm-cmat 20ºC
Magnetic Permeability 1.0081.008at RT
 
Thermal PropertiesMetricEnglishComments
CTE, linear  16.6 µm/m-°C
@Temperature 0.000 - 100 °C
9.22 µin/in-°F
@Temperature 32.0 - 212 °F
 17.5 µm/m-°C
@Temperature 0.000 - 315 °C
9.72 µin/in-°F
@Temperature 32.0 - 599 °F
 18.2 µm/m-°C
@Temperature 0.000 - 540 °C
10.1 µin/in-°F
@Temperature 32.0 - 1000 °F
Specific Heat Capacity 0.485 J/g-°C
@Temperature 0.000 - 100 °C
0.116 BTU/lb-°F
@Temperature 32.0 - 212 °F
Thermal Conductivity 14.4 W/m-K
@Temperature 100 °C
99.9 BTU-in/hr-ft²-°F
@Temperature 212 °F
Melting Point 1370 - 1400 °C2500 - 2550 °F
Solidus 1370 °C2500 °F
Liquidus 1400 °C2550 °F
Maximum Service Temperature, Air 870 °C1600 °FIntermittent
 925 °C1700 °FContinuous Service
 
Component Elements PropertiesMetricEnglishComments
Carbon, C <= 0.080 %<= 0.080 %
Chromium, Cr 16 - 18 %16 - 18 %
Iron, Fe 62.22 - 72.15 %62.22 - 72.15 %As Balance
Manganese, Mn <= 2.0 %<= 2.0 %
Molybdenum, Mo 1.75 - 2.5 %1.75 - 2.5 %
Nickel, Ni 10 - 14 %10 - 14 %
Phosphorus, P <= 0.20 %<= 0.20 %
Silicon, Si <= 1.0 %<= 1.0 %
Sulfur, S >= 0.10 %>= 0.10 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
AISI Type 430F Stainless Steel annealed bar
Schmolz + Bickenbach 416 Stainless Steel Bar
AISI Type 316F Stainless Steel, annealed sheet
AISI Type 316L Stainless Steel, annealed bar
414 Stainless Steel, annealed and cold drawn bar

MQ316M / 12800

Elmet Technologies

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.