System Message
Advertise with MatWeb!
Data sheets for over
180,000
metals, plastics, ceramics, and composites.
HOME
•
SEARCH
•
TOOLS
•
SUPPLIERS
•
FOLDERS
•
ABOUT US
•
FAQ
•
LOG IN
Recently Viewed Materials (most recent at top)
Login
to see your most recently viewed materials here.
Or if you don't have an account with us yet, then
click here to register.
Searches:
Advanced
|
Category
|
Property
|
Metals
|
Trade Name
|
Manufacturer
|
Recently Viewed Materials
Celanese Impet® 2700 GV1/30 PET, 30% Glass Reinforced
Categories:
Polymer
;
Thermoplastic
;
Polyester, TP
;
Polyethylene Terephthalate (PET)
;
Polyethylene Terephthalate (PET), 30% Glass Reinforced
Material Notes:
30% glass filled Polyethylene terephthalate (PET) with high flowability, excellent gloss, high modulus, and high heat deflection temperature.
Information provided by Celanese
Vendors:
No vendors are listed for this material. Please
click here
if you are a supplier and would like information on how to add your listing to this material.
Printer friendly version
Download as PDF
Download to Excel (requires Excel and Windows)
Export data to your CAD/FEA program
Add to Folder:
My Folder
Physical Properties
Metric
English
Comments
Density
1.60
g/cc
0.0578
lb/in³
ISO 1183
Moisture Absorption
0.150 %
0.150 %
23°C/50%RH; ISO 62
Viscosity Test
50
cm³/g
0.50
dl/g
ISO 307, 1157, 1628
Linear Mold Shrinkage, Flow
0.0090
cm/cm
0.0090
in/in
ISO 294-4
Linear Mold Shrinkage, Transverse
0.0070
cm/cm
0.0070
in/in
ISO 294-4
Mechanical Properties
Metric
English
Comments
Hardness, Rockwell M
123
123
ISO 2039-2
Tensile Strength at Break
168
MPa
24400
psi
5mm/min; ISO 527-2/1A
Elongation at Break
2.0 %
2.0 %
5mm/min; ISO 527-2/1A
Tensile Modulus
11.5
GPa
1670
ksi
50mm/min; ISO 527-2/1A
Flexural Strength
225
MPa
32600
psi
ISO 178
Flexural Modulus
11.1
GPa
1610
ksi
ISO 178
Izod Impact, Notched (ISO)
7.30
kJ/m²
3.47
ft-lb/in²
ISO 180/1A
Charpy Impact Unnotched
2.80
J/cm²
13.3
ft-lb/in²
ISO 179/1eU
2.80
J/cm²
@Temperature -30.0 °C
13.3
ft-lb/in²
@Temperature -22.0 °F
ISO 179/1eU
Charpy Impact, Notched
0.880
J/cm²
4.19
ft-lb/in²
ISO 179/1eA
0.880
J/cm²
@Temperature -30.0 °C
4.19
ft-lb/in²
@Temperature -22.0 °F
ISO 179/1eA
Electrical Properties
Metric
English
Comments
Volume Resistivity
2.00e+16
ohm-cm
2.00e+16
ohm-cm
IEC 60093
Surface Resistance
3.00e+15
ohm
3.00e+15
ohm
IEC 60093
Dielectric Constant
4.2
@Frequency 1e+6 Hz
4.2
@Frequency 1e+6 Hz
IEC 60250
4.8
@Frequency 100 Hz
4.8
@Frequency 100 Hz
IEC 60250
Dielectric Strength
33.0
kV/mm
838
kV/in
IEC 60243-1
Dissipation Factor
0.013
@Frequency 100 Hz
0.013
@Frequency 100 Hz
IEC 60250
0.018
@Frequency 1e+6 Hz
0.018
@Frequency 1e+6 Hz
IEC 60250
Comparative Tracking Index
170
V
170
V
IEC 60112
Thermal Properties
Metric
English
Comments
CTE, linear, Parallel to Flow
21.0
µm/m-°C
11.7
µin/in-°F
ISO 11359-2
CTE, linear, Transverse to Flow
64.0
µm/m-°C
35.6
µin/in-°F
ISO 11359-2
Melting Point
251
°C
484
°F
10°C/min; ISO 11357-1,-2,-3
Deflection Temperature at 0.46 MPa (66 psi)
252
°C
486
°F
ISO 75-1, -2
Deflection Temperature at 1.8 MPa (264 psi)
225
°C
437
°F
ISO 75-1, -2
Deflection Temperature at 8.0 MPa
135
°C
275
°F
ISO 75-1, -2
Vicat Softening Point
260
°C
500
°F
ISO 306
Glass Transition Temp, Tg
80.0
°C
176
°F
ISO 11357-1,-2,-3
Flammability, UL94
HB
@Thickness 1.60 mm
HB
@Thickness 0.0630 in
HB
@Thickness 0.800 mm
HB
@Thickness 0.0315 in
Oxygen Index
25 %
25 %
ISO 4589
Processing Properties
Metric
English
Comments
Processing Temperature
135
-
145
°C
275
-
293
°F
cavity
270
-
290
°C
518
-
554
°F
hot runner
Feed Temperature
40.0
-
60.0
°C
104
-
140
°F
Zone 1
260
-
270
°C
500
-
518
°F
Zone 2
270
-
280
°C
518
-
536
°F
Zone 3
280
-
290
°C
536
-
554
°F
Zone 4
280
-
290
°C
536
-
554
°F
Die Temperature
270
-
290
°C
518
-
554
°F
Melt Temperature
270
-
290
°C
518
-
554
°F
Drying Temperature
120
-
140
°C
248
-
284
°F
Dry Time
2.00
-
4.00
hour
2.00
-
4.00
hour
Moisture Content
<= 0.010 %
<= 0.010 %
Screw Speed
50
rpm
@Diameter 55.0 mm
50
rpm
@Diameter 2.17 in
65
rpm
@Diameter 40.0 mm
65
rpm
@Diameter 1.57 in
80
rpm
@Diameter 25.0 mm
80
rpm
@Diameter 0.984 in
Descriptive Properties
Injection molding
Yes
Injection speed
fast
pvT (Generic Grade reference)
PET-09-110, GF30
Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's
terms of use
regarding this information.
Click here
to view all the property values for this datasheet as they were originally entered into MatWeb.
Users viewing this material also viewed the following:
EMS-Grivory Grivory® HT2V-3X V0 black 9021 PA6T/66-GF30
Celanese Hostaform® C 9021 GV1/30 POM, 30% Glass Reinforced
Celanese Impet® 2700 GV1/45 (Europe) PET, 45% Glass Reinforced
LATI Latan 13 G/30 POM, 30% Glass Fiber Reinforced
Celanese Hostaform® C 27021 GV3/30 POM, 30% Glass Reinforced
PHCQ441 / 178896
Subscribe to Premium Services
Searches:
Advanced
•
Composition
•
Property
•
Material Type
•
Manufacturer
•
Trade Name
•
UNS Number
Other Links:
Advertising
•
Submit Data
•
Database Licensing
•
Web Design & Hosting
•
Trade Publications
Supplier List
•
Unit Converter
•
Reference
•
Links
•
Help
•
Contact Us
•
Site Map
•
FAQ
•
Home
Follow @MatWeb
Please read our
License Agreement
regarding materials data and our
Privacy Policy
. Questions or comments about MatWeb? Please contact us at
info@matweb.com
. We appreciate your input.
The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.