MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

LyondellBasell Pro-fax™ SG899 Polypropylene Copolymer
Categories: Polymer; Thermoplastic; Polypropylene (PP); Polypropylene Copolymer

Material Notes: Description: Pro-fax™ SG899 high flow, high impact polypropylene copolymer resin is tailored for use in automotive interior head impact applications. This resin is designed to be run in conventional injection molding equipment using standard polypropylene processing conditions. It is available in pellet form. All ingredients in Pro-fax™ SG899 resin meet the chemical registration requirements of TSCA (U.S.) and DSL (Canada). Uses: Automotive interior parts

Information provided by Basell.

Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 0.900 g/cc0.0325 lb/in³ASTM D792 & ISO 1183
Melt Flow 35 g/10 min
@Load 2.16 kg,
Temperature 230 °C
35 g/10 min
@Load 4.76 lb,
Temperature 446 °F
Condition L; ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Yield 21.4 MPa3100 psiASTM D 638
 22.0 MPa3190 psiISO 527-1, -2
Elongation at Break 50 %50 %ISO 527-1, -2
Elongation at Yield 5.0 %5.0 %ISO 527-1, -2
 6.0 %6.0 %ASTM D 638
Flexural Modulus 1.10 GPa160 ksiISO 178
Flexural Modulus, 1% Secant 1030 MPa150000 psi0.05 in/min; ASTM D790
Izod Impact, Notched 2.99 J/cm5.60 ft-lb/in73°F; ASTM D256
Izod Impact, Notched (ISO)  5.50 kJ/m²
@Temperature -40.0 °C
2.62 ft-lb/in²
@Temperature -40.0 °F
ISO 180
 7.50 kJ/m²
@Temperature -18.0 °C
3.57 ft-lb/in²
@Temperature -0.400 °F
ISO 180
 14.0 kJ/m²
@Temperature 23.0 °C
6.66 ft-lb/in²
@Temperature 73.4 °F
ISO 180
 
Thermal PropertiesMetricEnglishComments
Deflection Temperature at 0.46 MPa (66 psi) 87.8 °C190 °FUnannealed; ISO 75B-1, -2
 97.8 °C208 °FUnannealed; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 52.2 °C126 °FUnannealed; ISO 75A-1, -2

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Phillips Sumika Marlex® AGM-250 Polypropylene Impact Copolymer, Ultra-low temperature, impact-resistant, reactor TPO
LyondellBasell Pro-fax 7624 Polypropylene Impact Copolymer, Heat- and Extraction-Resistant
LyondellBasell Pro-fax SV258 Polypropylene Impact Copolymer
A. Schulman POLYTROPE™ TPP 504 Injection Molding Grade Olefinic Thermoplastic Elastomer
Dow Engage® 8003 Polyolefin Elastomer

PMO887 / 53876

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.