MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
INEOS Styrolution Lustran® 248FC Acrylonitrile Butadiene Styrene (ABS)
Categories: Polymer; Thermoplastic; ABS Polymer; Acrylonitrile Butadiene Styrene (ABS), Molded

Material Notes: Lustran® 248FC resin is a high-gloss, medium-impact grade of ABS (acrylonitrile butadiene styrene). Healthcare certifications, High Gloss, Medium impact, Compliant with both food and medical regulations. Applications: Components of intravenous (IV)systems, Surgical instruments, Diagnostic test kits

Information provided by Styrolution.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.06 g/ccASTM D 792
Linear Mold Shrinkage 0.0040 - 0.0060 cm/cmASTM D 955
Melt Flow 5.0 g/10 min
@Load 3.80 kg,
Temperature 230 °C
ASTM D 1238
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell R 112ASTM D 785
Tensile Strength, Yield 46.9 MPaASTM D 638
Tensile Modulus 2620 MPaASTM D 638
Flexural Strength 73.8 MPaASTM D 790
Flexural Modulus 2690 MPaASTM D 790
Izod Impact, Notched 4.20 ft-lb/in
@Temperature 23.0 °C
ASTM D 256
 
Thermal PropertiesOriginal ValueComments
Deflection Temperature at 0.46 MPa (66 psi) 100 °Cannealed; ASTM D 648
Deflection Temperature at 1.8 MPa (264 psi) 86.0 °Cunannealed; ASTM D 648
 95.6 °Cannealed; ASTM D 648
 
Processing PropertiesOriginal ValueComments
Melt Temperature 218 - 260 °C
Mold Temperature 29.0 - 60.0 °C
Drying Temperature 79.0 °C
@Time 7200 - 14400 sec

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Trinseo MAGNUM™ 3904 Acrylonitrile Butadiene Styrene (ABS) Resin
Overview of materials for Polycarbonate/ABS Alloy, Carbon Fiber Filled
Overview of materials for Acrylonitrile Butadiene Styrene (ABS)/Nylon Blend
Mitsubishi Chemical Advanced Materials Ertalyte™ PET Polyester-semi-crystalline thermoplastic, extruded
INEOS Styrolution Lustran® 620 Acrylonitrile Butadiene Styrene (ABS)

PSTYR9849 / 216076

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.