MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Dow PELLETHANE® 2355-55DE Polyurethane Elastomer, Polyester Polyadipate Based  (discontinued **)
Categories: Polymer; Thermoplastic; Elastomer, TPE; Polyurethane, TP; Thermoplastic Polyurethane, Elastomer, Polyester Grade

Material Notes: Description: PELLETHANE® 2355-55DE polyester polyadipate based polyurethane elastomer has excellent oil and chemical resistance. Applications include: Film, Sheet, Tubing, Recreation and sporting equipment, Industrial hoses, Fabric lamination, Sewer pipe linings, Footwear

Data provided by Dow Chemical.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.19 g/ccASTM D792
Linear Mold Shrinkage 0.0090 - 0.013 cm/cm
@Thickness 1.59 mm
plaque
Melt Index of Compound 24 g/10 min
@Load 8.70 kg,
Temperature 190 °C
ASTM D1238
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore D 49 - 57ASTM D2240
Tensile Strength, Ultimate 41.4 MPaASTM D412
Elongation at Break 500 %ASTM D412
50% Modulus 0.00930 GPa
@Strain 50 %
ASTM D412
100% Modulus 0.0121 GPa
@Strain 100 %
ASTM D412
300% Modulus 0.0248 GPa
@Strain 300 %
ASTM D412
Flexural Modulus 24000 psiASTM D790
Tear Strength 114 kN/mDie C; ASTM D624
Taber Abrasion, mg/1000 Cycles 60H-22 wheel (coarser); ASTM D1044
Compression Set 35 %
@Temperature 70.0 °C
22 hrs.; ASTM D395, Method B
 25 %
@Temperature 25.0 °C,
Time 79200 sec
ASTM D395, Method B
Tensile Set 80 %Elongation Set After Break; ASTM D412
 
Thermal PropertiesOriginal ValueComments
Vicat Softening Point 107 °CASTM D1525
 
Processing PropertiesOriginal ValueComments
Processing Temperature 199 - 216 °COptimum Extrusion Temperature
Melt Temperature 204 - 221 °C

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Dow PELLETHANE® 2104-65D Polyurethane Elastomer (Ether-Ether Hybrid)
Dow PELLETHANE® 2103-75D Film Grade Thermoplastic Polyurethane Elastomer
Dow Pellethane® 2354-65D Polyurethane Elastomer, Polyester Polycaprolactone Based
Lubrizol Pellethane® 2363-90A Thermoplastic Polyurethane Elastomer
Covestro Makroblend® UT-403 Polycarbonate + Polyester Blend

PDW300 / 34468

Polyurethane

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.