MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Metalmen Sales

(Viewing data as-entered. Click here to return)
AK Steel NITRONIC® 30 Austenitic Stainless Steel
Categories: Metal; Ferrous Metal; Stainless Steel

Material Notes: AK Steel NITRONIC 30 Stainless Steel offers significantly higher strength than Type 304 and potential for applications requiring good resistance to aqueous and atmospheric corrosion resistance combined with good toughness and economy. Specific potential applications include automotive hose clamps, safety belt anchors, truck and bus frames, water supply and control structures, sewage treatment plant structures, bulk solids handling equipment, magnetic ore separator screens, coal buckets and hopper cars. Stainless steels have served successfully in many structural components in the transportation industry. Bus space frames and bumpers take advantage of the excellent fabricability and high strength and toughness of stainless steel. Tensilized NITRONIC 30 Stainless Steel has been used in rapid transit structurals where the strength-to-weight ratio of up to three times that of carbon steel has improved operating efficiency. Rear frames of refrigerated trucks are easily welded and formed from NITRONIC 30 Stainless Steel, resulting in protective units that can withstand impact blows without cracking. Shipboard container structurals use stainless steel successfully where carbon steel becomes scuffed and rusts wherever the paint is damaged.

AK Steel NITRONIC 30 is a nitrogen-strengthened stainless steel developed for applications requiring a good level of aqueous corrosion resistance combined with good toughness and economy. AK Steel NITRONIC 30 Stainless Steel provides approximately 50% higher yield strength than Type 304L and, therefore, may allow lighter gauges to further reduce costs. AK Steel NITRONIC 30 Stainless Steel work hardens rapidly while retaining good ductility. Unlike other nitrogen-strengthened stainless steels, AK Steel NITRONIC 30 Stainless Steel is subject to magnetic transformation when cold worked.

Information provided by AK Steel

Key Words: UNS S20400
Vendors: Visit metalmen for your metals needs. Products include special chemistry, tight tolerances, custom tempers, odd dimensions/forms, and small quantities. Phone 1-800-767-9494.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 7.86 g/ccBased on UNS number
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell B 950% Cold Work
 92.5
@Temperature 23.9 °C
Plate
 96.5
@Temperature 23.9 °C
 92
@Thickness 22.2 mm
Typical for Plate, Annealed, in 2"
 93
@Thickness 1.63 mm
Annealed at 2050°F, Longitudinal
 93
@Thickness 1.63 mm
Annealed at 2050°F, Transverse
 93.5
@Thickness 3.15 mm
Annealed at 1950°F, Longitudinal
 94
@Thickness 9.52 mm
Typical for Plate, Annealed
 94
@Thickness 0.813 mm
Annealed at 1950°F, Longitudinal
 94
@Thickness 0.813 mm
Annealed at 1950°F, Longitudinal
Hardness, Rockwell C 3110% Cold Work
 3720% Cold Work
 4330% Cold Work
 4540% Cold Work
 33.5
@Thickness 4.762 mm
Typical for Plate, 1/4-Hard, Longitudinal
 33.5
@Thickness 4.762 mm
Typical for Plate, 1/4-Hard, Transverse
 34
@Thickness 6.35 mm
Typical for Plate, 1/4-Hard, Longitudinal
 34
@Thickness 6.35 mm
Typical for Plate, 1/4-Hard, Transverse
Tensile Strength, Ultimate 862 MPa0% Cold Work
 1034 MPa10% Cold Work
 1193 MPa20% Cold Work
 1338 MPa30% Cold Work
 1467 MPa40% Cold Work
 66.5 ksi
@Temperature 538 °C
Sheet
 70.3 ksi
@Temperature 482 °C
Sheet
 73.4 ksi
@Temperature 427 °C
Sheet
 76.7 ksi
@Temperature 371 °C
Sheet
 79.3 ksi
@Temperature 316 °C
Sheet
 79.3 ksi
@Temperature 260 °C
Sheet
 81.4 ksi
@Temperature 204 °C
Sheet
 86.8 ksi
@Temperature 149 °C
Sheet
 100 ksi
@Temperature 93.3 °C
Sheet
 123 ksi
@Temperature 23.9 °C
Sheet
 417 MPa
@Temperature 538 °C
Plate
 439 MPa
@Temperature 482 °C
Plate
 460 MPa
@Temperature 427 °C
Plate
 480 MPa
@Temperature 371 °C
Plate
 487 MPa
@Temperature 260 °C
Plate
 488 MPa
@Temperature 316 °C
Plate
 496 MPa
@Temperature 204 °C
Plate
 539 MPa
@Temperature 149 °C
Plate
 630 MPa
@Temperature 93.3 °C
Plate
 850 MPa
@Temperature 23.9 °C
Plate
 689 MPa
@Thickness 1.63 mm
Annealed at 2050°F, Longitudinal
 711 MPa
@Thickness 1.63 mm
Annealed at 2050°F, Transverse
 786 MPa
@Thickness 9.52 mm
Typical for Plate, Annealed
 811 MPa
@Thickness 3.15 mm
Annealed at 1950°F, Longitudinal
 825 MPa
@Thickness 0.813 mm
Annealed at 1950°F, Longitudinal
 827 MPa
@Thickness 50.8 mm
Typical for Plate, Annealed
 840 MPa
@Thickness 0.813 mm
Annealed at 1950°F, Longitudinal
 855 MPa
@Thickness 22.2 mm
Typical for Plate, Annealed
 998 MPa
@Thickness 6.35 mm
Typical for Plate, 1/4-Hard, Longitudinal
 1011 MPa
@Thickness 6.35 mm
Typical for Plate, 1/4-Hard, Transverse
 1020 MPa
@Thickness 4.762 mm
Typical for Plate, 1/4-Hard, Longitudinal
 1025 MPa
@Thickness 4.762 mm
Typical for Plate, 1/4-Hard, Transverse
Tensile Strength, Yield 345 MPa
@Strain 0.2 %
Typical for Plate, Annealed, 0.875"
 358 MPa
@Strain 0.2 %
Typical for Plate, Annealed, 2"
 393 MPa
@Strain 0.2 %
Typical for Plate, Annealed, 0.0375"
 393 MPa
@Strain 0.2 %
0% Cold Work
 593 MPa
@Strain 0.2 %
10% Cold Work
 702 MPa
@Strain 0.2 %
Typical for Plate, 1/4-Hard, Longitudinal, 0.25"
 717 MPa
@Strain 0.2 %
Typical for Plate, 1/4-Hard, Longitudinal, 0.1875'
 759 MPa
@Strain 0.2 %
Typical for Plate, 1/4-Hard, Transverse, 0.25"
 768 MPa
@Strain 0.2 %
Typical for Plate, 1/4-Hard, Transverse, 0.1875"
 779 MPa
@Strain 0.2 %
20% Cold Work
 979 MPa
@Strain 0.2 %
30% Cold Work
 1186 MPa
@Strain 0.2 %
40% Cold Work
 27.1 ksi
@Strain 0.2 %,
Temperature 538 °C
Sheet
 28.6 ksi
@Strain 0.2 %,
Temperature 482 °C
Sheet
 30.0 ksi
@Strain 0.2 %,
Temperature 427 °C
Sheet
 33.8 ksi
@Strain 0.2 %,
Temperature 316 °C
Sheet
 34.9 ksi
@Strain 0.2 %,
Temperature 260 °C
Sheet
 37.6 ksi
@Strain 0.2 %,
Temperature 204 °C
Sheet
 41.1 ksi
@Strain 0.2 %,
Temperature 149 °C
Sheet
 47.3 ksi
@Strain 0.2 %,
Temperature 93.3 °C
Sheet
 63.1 ksi
@Strain 0.2 %,
Temperature 23.9 °C
Sheet
 131 MPa
@Strain 0.2 %,
Temperature 538 °C
Plate
 155 MPa
@Strain 0.2 %,
Temperature 482 °C
Plate
 157 MPa
@Strain 0.2 %,
Temperature 427 °C
Plate
 168 MPa
@Strain 0.2 %,
Temperature 371 °C
Plate
 174 MPa
@Strain 0.2 %,
Temperature 316 °C
Plate
 182 MPa
@Strain 0.2 %,
Temperature 260 °C
Plate
 190 MPa
@Strain 0.2 %,
Temperature 204 °C
Plate
 217 MPa
@Strain 0.2 %,
Temperature 371 °C
Sheet
 222 MPa
@Strain 0.2 %,
Temperature 149 °C
Plate
 266 MPa
@Strain 0.2 %,
Temperature 93.3 °C
Plate
 362 MPa
@Strain 0.2 %,
Temperature 23.9 °C
Plate
 368 MPa
@Strain 0.2 %,
Thickness 1.63 mm
Annealed at 2050°F, Transverse
 370 MPa
@Strain 0.2 %,
Thickness 1.63 mm
Annealed at 2050°F, Longitudinal
 372 MPa
@Strain 0.2 %,
Thickness 3.15 mm
Annealed at 1950°F, Longitudinal
 375 MPa
@Strain 0.2 %,
Thickness 0.813 mm
Annealed at 1950°F, Longitudinal
 379 MPa
@Strain 0.2 %,
Thickness 0.813 mm
Annealed at 1950°F, Longitudinal
Elongation at Break 15 %In 2", 40% Cold Work
 18 %In 2", 30% Cold Work
 25 %In 2", 20% Cold Work
 35 %In 2",10% Cold Work
 49 %In 2", 0% Cold Work
 42.9 %
@Temperature 538 °C
In 2", Plate
 46.4 %
@Temperature 316 °C
In 2", Plate
 47.7 %
@Temperature 482 °C
In 2", Plate
 48 %
@Temperature 204 °C
In 2", Plate
 48.3 %
@Temperature 427 °C
In 2", Plate
 48.6 %
@Temperature 260 °C
In 2", Plate
 49 %
@Temperature 371 °C
In 2", Plate
 50 %
@Temperature 23.9 °C
In 2", Plate
 65.5 %
@Temperature 149 °C
In 2", Plate
 77.8 %
@Temperature 93.3 °C
In 2", Plate
 29.6 %
@Thickness 6.35 mm
In 2", Typical for Plate, 1/4-Hard, Transverse
 31.5 %
@Thickness 4.762 mm
In 2", Typical for Plate, 1/4-Hard, Transverse
 35.5 %
@Thickness 4.762 mm
In 2", Typical for Plate, 1/4-Hard, Longitudinal
 35.5 %
@Thickness 6.35 mm
In 2", Typical for Plate, 1/4-Hard, Longitudinal
 31 - 40 %
@Thickness 50.8 mm
Typical, (Gauge, 0.028" -0.084")
 50 %
@Thickness 22.2 mm
In 2", Typical for Plate, Annealed
 52 %
@Thickness 3.15 mm
In 2", Annealed at 1950°F, Longitudinal
 54 %
@Thickness 0.813 mm
In 2", Annealed at 1950°F, Longitudinal
 54 %
@Thickness 50.8 mm
In 2", Typical for Plate, Annealed
 55 %
@Thickness 0.813 mm
In 2", Annealed at 1950°F, Longitudinal
 56 %
@Thickness 9.52 mm
In 2", Typical for Plate, Annealed
 58 %
@Thickness 1.63 mm
In 2", Annealed at 2050°F, Transverse
 58.5 %
@Thickness 1.63 mm
In 2", Annealed at 2050°F, Longitudinal
 34.1 %
@Thickness 50.8 mm,
Temperature 538 °C
in 2", Sheet
 40.7 %
@Thickness 50.8 mm,
Temperature 482 °C
in 2", Sheet
 41.30 %
@Thickness 50.8 mm,
Temperature 260 °C
in 2", Sheet
 41.30 %
@Thickness 50.8 mm,
Temperature 316 °C
in 2", Sheet
 43.7 %
@Thickness 50.8 mm,
Temperature 427 °C
in 2", Sheet
 44.3 %
@Thickness 50.8 mm,
Temperature 371 °C
in 2", Sheet
 44.8 %
@Thickness 50.8 mm,
Temperature 204 °C
in 2", Sheet
 46.8 %
@Thickness 50.8 mm,
Temperature 23.9 °C
in 2", Sheet
 53.7 %
@Thickness 50.8 mm,
Temperature 149 °C
in 2", Sheet
 63.3 %
@Thickness 50.8 mm,
Temperature 93.3 °C
in 2", Sheet
Charpy Impact, Unnotched 217 ft-lbTypical for Plate, Annealed
Charpy Impact, Notched 108.2 J/cm²
@Thickness 2.84 mm,
Temperature -101 °C
Base Metal
 128.4 J/cm²
@Thickness 2.84 mm,
Temperature 0.000 °C
Base Metal
 133.7 J/cm²
@Thickness 2.84 mm,
Temperature 23.9 °C
Base Metal
 
Thermal PropertiesOriginal ValueComments
CTE, linear 9.35 µin/in-°F
@Temperature 26.1 - 93.3 °C
 9.60 µin/in-°F
@Temperature 26.1 - 149 °C
 9.81 µin/in-°F
@Temperature 26.1 - 204 °C
 10.0 µin/in-°F
@Temperature 26.1 - 260 °C
 10.2 µin/in-°F
@Temperature 26.1 - 316 °C
 10.4 µin/in-°F
@Temperature 26.1 - 371 °C
 10.5 µin/in-°F
@Temperature 26.1 - 427 °C
 10.6 µin/in-°F
@Temperature 26.1 - 482 °C
 10.8 µin/in-°F
@Temperature 26.1 - 538 °C
 10.9 µin/in-°F
@Temperature 26.1 - 593 °C
 11.0 µin/in-°F
@Temperature 26.1 - 649 °C
 11.1 µin/in-°F
@Temperature 26.1 - 704 °C
 11.21 µin/in-°F
@Temperature 26.1 - 760 °C
 11.31 µin/in-°F
@Temperature 26.1 - 816 °C
 11.42 µin/in-°F
@Temperature 26.1 - 871 °C
 
Component Elements PropertiesOriginal ValueComments
Carbon, C <= 0.030 %
Chromium, Cr 15 - 17 %
Copper, Cu <= 1.0 %
Iron, Fe 68.6 - 76.35 %Balance
Manganese, Mn 7.0 - 9.0 %
Nickel, Ni 1.5 - 3.0 %
Nitrogen, N 0.15 - 0.30 %
Phosphorus, P <= 0.040 %
Silicon, Si <= 1.0 %
Sulfur, S <= 0.030 %
 
Descriptive Properties
'n' Value0.19Strain Hardening Coefficient, Typical, (Gauge, 0.028" -0.084")
Olsen Cup Height0.330"-0.450"Typical, (Gauge, 0.028" -0.084")

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
AK Steel 201 Austenitic Stainless steel
ATI Allegheny Ludlum Stainless Steel Type 201L, 10% Cold Work (UNS S20103)
AK Steel 201LN Austenitic Stainless steel
ATI Allegheny Ludlum Stainless Steel Type 201, 20% Cold Work (UNS S20100)
ATI Allegheny Ludlum Stainless Steel Type 301, 1/2 Hard (UNS S30100)

NAKS141 / 138556

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.