MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
BASF Ultramid® HMG14 HS BK 102 60% Glass Filled PA66 (Conditioned)
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 66 (PA66); Nylon 66, 60% Glass Fiber Filled

Material Notes: Description: Ultramid HMG14 HS BK-102 is a 60% glass reinforced, injection molding grade of PA66 offering high strength and stiffness. Due to inherently lower moisture absorption, Ultramid HMG14 HS BK-102 shows improved retention of mechanical properties after moisture conditioning. In addition, molded parts possess an exceptional surface finish.

Applications: Ultramid HMG14 HS BK-102 was designed for applications requiring very high rigidity and should be considered for components that are constructed with metal.

Information provided by BASF

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.75 g/ccISO 1183
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 220 MPaISO 527
Tensile Modulus 20830 MPaISO 527
Flexural Strength 351 MPaISO 178
Flexural Modulus 19400 MPaISO 178
Izod Impact, Notched (ISO) 11.0 kJ/m²ISO 180
 13.0 kJ/m²ISO 180
Charpy Impact Unnotched 85.0 kJ/m²
@Temperature -30.0 °C
ISO 179
 93.0 kJ/m²
@Temperature 23.0 °C
ISO 179
Charpy Impact, Notched 12.0 kJ/m²
@Temperature -30.0 °C
ISO 179
 15.0 kJ/m²
@Temperature 23.0 °C
ISO 179
 
Processing PropertiesOriginal ValueComments
Melt Temperature 280 - 305 °C
Mold Temperature 80.0 - 90.0 °C
Dry Time 2 - 4 hour
Moisture Content <= 0.12 %
 
Descriptive Properties
ColorBK 102
Commercial StatusNorth America

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
BASF Ultramid® HMG14 HS BK 102 60% Glass Filled PA66 (Dry)
BASF Ultramid® A3EG3 15% Glass Filled PA66 (Conditioned)
BASF Ultramid® A3EG10 50% Glass Filled PA66 (Conditioned)
Overview of materials for Nylon 6, 40% Glass Fiber Filled
BASF Ultramid® A3EG3 15% Glass Filled PA66 (Dry)

PBASG0462 / 132095

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.