MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Baystar™ Lumicene® mPE M 2710 EP Metallocene Medium Density Polyethylene Film Resin
Categories: Polymer; Film; Thermoplastic; Polyethylene (PE); High Density (HDPE); Medium Density (MDPE); Medium Density Polyethylene (MDPE), Film Grade

Material Notes: Metallocene Medium Density Film Resin

Characteristics:

  • Outstanding clarity and gloss
  • Excellent bubble stability
  • Excellent tear strength
  • High puncture resistance
  • Good stiffness
  • Excellent heat sealing properties
  • Excellent compatibility with LDPE and LLDPE

Applications:

  • Clarity shrink films
  • Food packaging
  • Laminations and multilayer packaging films
  • Machine direction oriented (MDO) films
Film was produced at 1.0 mil with a 2.5:1 BUR

This former Total Petrochemicals grade is now a part of the Bayport Polymers joint venture in the Americas.

Key Words: Outstanding clarity and gloss; Excellent bubble stability
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.927 g/ccASTM D-792
Water Vapor Transmission 0.900 g/100 in²/dayASTM F-1294
Melt Flow 0.90 g/10 min
@Load 2.16 kg,
Temperature 190 °C
ASTM D-1238
High Load Melt Index 30 g/10 min
@Load 21.6 kg,
Temperature 190 °C
ASTM D-1238
 
Mechanical PropertiesOriginal ValueComments
Film Elongation at Break, MD 580 %ASTM D-882, A
Film Elongation at Break, TD 720 %ASTM D-882, A
Elmendorf Tear Strength MD 165 gASTM D1922
Elmendorf Tear Strength TD 500 gASTM D1922
Dart Drop Test 150 gASTM D1709, A
Film Tensile Strength at Break, MD 4900 psiASTM D-882, A
Film Tensile Strength at Break, TD 4800 psiASTM D-882, A
1% Secant Modulus, MD 31000 psiASTM D-882, A
1% Secant Modulus, TD 25000 psiASTM D-882, A
 
Thermal PropertiesOriginal ValueComments
Melting Point 250 °FASTM D-3417
 
Optical PropertiesOriginal ValueComments
Haze 7.00 %ASTM D1003
Gloss 65.0 %45°; ASTM D2457
 
Descriptive Properties
ProcessFilm

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Overview of materials for Low Density Polyethylene (LDPE), Film Grade
A. Schulman POLYBATCH™ FSU-105-E Concentrate Based In LDPE
ExxonMobil Exceed™ Flow m 0527.MC Film Grade Hexene LLDPE
ExxonMobil Exceed™ Flow m 0535.MC Blown Film Grade Hexene LLDPE
Braskem LD7001A Coextruded and Shrink Films Low Density Polyethylene

PBAYST909 / 130498

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.