MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
ExxonMobil LD 144.50 Packaging Film Resin  (discontinued **)
Categories: Polymer; Film; Thermoplastic; Ethylene Vinyl Acetate; Ethylene Vinyl Acetate Copolymer (EVA), Film Grade

Material Notes: Film made from LD 144.50 offers improved impact strength and heat sealability compared to homopolymer clarity film resins. Typically applications include food packaging, frozen food packaging, and textile goods packaging rack and counter bags.

Information provided by ExxonMobil Chemical

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.921 g/ccExxonMobil Method
Vinyl Acetate Content 2.0 %ExxonMobil Method
Melt Flow 2.0 g/10 minExxonMobil Method
Antiblock Level 3500 ppm
Slip Level 725 ppm
 
Mechanical PropertiesOriginal ValueComments
Film Tensile Strength at Yield, MD 1320 psiat 2% offset; ASTM D882
Film Tensile Strength at Yield, TD 1330 psiat 2% offset; ASTM D882
Film Elongation at Break, MD 160 %ASTM D882
Film Elongation at Break, TD 550 %ASTM D882
Film Elongation at Yield, MD 6.4 %ASTM D882
Film Elongation at Yield, TD 5.5 %ASTM D882
Elmendorf Tear Strength MD 310 gASTM D1922
Elmendorf Tear Strength TD 100 gASTM D1922
Dart Drop Test 140 gASTM D1709
Film Tensile Strength at Break, MD 3440 psiASTM D882
Film Tensile Strength at Break, TD 3000 psiASTM D882
1% Secant Modulus, MD 24900 psiASTM D882
1% Secant Modulus, TD 30100 psiASTM D882
 
Thermal PropertiesOriginal ValueComments
Melting Point 224 °FPeak Melting Temperature; ExxonMobil Method
Crystallization Temperature 94.0 °CExxonMobil Method
Vicat Softening Point 194 °FASTM D1525
 
Optical PropertiesOriginal ValueComments
Haze 8.1 %ASTM D1003
Gloss 63 %45°; ASTM D2457
 
Descriptive Properties
FeaturesThermal Stabilizer

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
ExxonMobil Escorene® LD 705.MJ Molding, extrusion and compounding resin
ExxonMobil LD 141.87 Shrink Film Resin
LyondellBasell Petrothene® NA426225 Low Density Polyethylene, Film Extrusion Grade
Dow Elvax® 40L-03 Ethylene-Vinyl Acetate Copolymer Resin
ExxonMobil Escorene® UL 7765 Adhesive Application Resin

PEXB001 / 37306

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.