MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

(Viewing data as-entered. Click here to return)
ExxonMobil Santoprene® 121-87 Thermoplastic Elastomer
Categories: Polymer; Thermoplastic; Elastomer, TPE; Thermoplastic Vulcanizate Elastomer (TPV)

Material Notes: A hard, black, UV resistant thermoplastic vulcanizate (TPV) in the thermoplastic elastomer (TPE) family. This material combines good physical properties and chemical resistance for use in a wide range of applications. This grade of Santoprene TPV is shear-dependent and can be processed on conventional thermoplastics equipment for injection molding, extrusion or blow molding. It is polyolefin based and completely recyclable.

Key Features:

  • Recommended for applications requiring excellent flex fatigue resistance.
  • Excellent ozone resistance.
  • Designed for improved UV resistance.
  • Although not NSF certified, this product has a Material Supplier Form on file with NSF to facilitate its evaluation for use in applications requiring NSF certification.
  • EU and China RoHS compliant.
Applications:
  • Automotive- Interior Mat, Seals, Gaskets and Weather Seals
Uses:
  • Automotive Applications
  • Automotive Interior Trim
  • Automotive Exterior Trim
  • Automotive Under the Hood
Availability: Africa & Middle East, Europe, North America, Asia Pacific, Latin America and South America

Information provided by ExxonMobil Chemical

Key Words: EU 2003/11/EC; RoHS Compliant
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 0.970 g/ccASTM D792
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 932 mm, 15 sec; ISO 868
 94Air at 275°F, 1008 hr; ASTM D573
Tensile Strength at Break 2134 psiAir at 275°F, 1008 hr; ASTM D573
 2200 psiAcross Flow; ASTM D412
Tensile Stress at Strain 986 psi
@Strain 100 %
Across Flow; ASTM D412
Elongation at Break 490.2 %Air at 275°F, 1008 hr; ASTM D573
 570 %Across Flow; ASTM D412
Tear Strength 286 pli73°F, Die C; ASTM D624
Compression Set 28 %
@Temperature 22.8 °C,
Time 79200 sec
ASTM D395
 65 %
@Temperature 125 °C,
Time 252000 sec
ASTM D395
 
Electrical PropertiesOriginal ValueComments
Dielectric Constant 2.71.98 mm; ASTM D150
Dielectric Strength 670 V/mil2.03 mm; ASTM D149
 
Thermal PropertiesOriginal ValueComments
Maximum Service Temperature, Air 275 °F
Brittleness Temperature -72.0 °FASTM D746
 
Processing PropertiesOriginal ValueComments
Processing Temperature 175 - 230 °C
Rear Barrel Temperature 360 °F
Middle Barrel Temperature 370 °F
Front Barrel Temperature 380 °F
Nozzle Temperature 390 - 455 °F
Die Temperature 410 °FExtrusion
Melt Temperature 400 °FExtrusion
 400 - 450 °FProcessing
Mold Temperature 50.0 - 125 °FProcessing
Drying Temperature 180 °F
Dry Time 3 hour
Moisture Content 0.080 %
Back Pressure 50.0 - 100 psiProcessing
 725 - 2900 psiExtrusion
Clamp Pressure 6000 - 10000 psi
Vent Depth 0.00100 in
Cushion 0.125 - 0.250 in
Screw Speed 100 - 200 rpm
 
Descriptive Properties
ColorBlack
FormPellets
Injection RateFast
Maximum Regrind %20
Screw Compression Ratio2:1 - 2.5:1
Screw L/D Ratio16:1 - 20:1

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Advanced Elastomer Systems Santoprene® 281-87 Thermoplastic Rubber
ExxonMobil Santoprene® 111-87 Thermoplastic Elastomer
ExxonMobil Santoprene® 101-87 Thermoplastic Elastomer
ExxonMobil Santoprene® 8201-80 Thermoplastic Elastomer
Covestro Makroblend® KU 2-7912 Polycarbonate + PBT, Impact Grade

PADVA074 / 22764

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.