Physical Properties | Metric | English | Comments |
---|
Specific Gravity | 1.51 g/cc | 1.51 g/cc |
Density | 1.49 g/cc | 0.0538 lb/in³ |
Filler Content | 30 % | 30 % |
Moisture Absorption | 0.060 % @Temperature 23.0 °C | 0.060 % @Temperature 73.4 °F |
Linear Mold Shrinkage | 0.0063 cm/cm @Thickness 1.60 mm | 0.0063 in/in @Thickness 0.0630 in |
| 0.0075 cm/cm @Thickness 3.20 mm | 0.0075 in/in @Thickness 0.126 in |
Linear Mold Shrinkage, Flow | 0.0035 cm/cm | 0.0035 in/in |
| 0.0020 cm/cm @Thickness 3.20 mm | 0.0020 in/in @Thickness 0.126 in |
| 0.0021 cm/cm @Thickness 1.60 mm | 0.0021 in/in @Thickness 0.0630 in |
| 0.0025 cm/cm @Thickness 2.00 mm | 0.0025 in/in @Thickness 0.0787 in |
Linear Mold Shrinkage, Transverse | 0.0105 cm/cm | 0.0105 in/in |
| 0.0085 cm/cm @Thickness 2.00 mm | 0.0085 in/in @Thickness 0.0787 in |
Melt Index of Compound | 5.5 g/10 min @Load 5.00 kg, Temperature 280 °C | 5.5 g/10 min @Load 11.0 lb, Temperature 536 °F |
|
Mechanical Properties | Metric | English | Comments |
---|
Hardness, Rockwell M | 70 | 70 |
| 70 | 70 |
Hardness, Rockwell R | 115 | 115 |
| 115 | 115 |
Tensile Strength at Break | 125 MPa @Temperature 23.0 °C | 18100 psi @Temperature 73.4 °F |
Tensile Strength | 126 MPa @Temperature 23.0 °C | 18300 psi @Temperature 73.4 °F |
Elongation at Break | 3.3 % @Temperature 23.0 °C | 3.3 % @Temperature 73.4 °F |
| 3.3 % @Temperature 23.0 °C | 3.3 % @Temperature 73.4 °F |
Tensile Modulus | 9.30 GPa @Temperature 23.0 °C | 1350 ksi @Temperature 73.4 °F |
| 9.31 GPa @Temperature 23.0 °C | 1350 ksi @Temperature 73.4 °F |
Flexural Strength | 193 MPa @Temperature 23.0 °C | 28000 psi @Temperature 73.4 °F |
Flexural Modulus | 7.83 GPa @Temperature 23.0 °C | 1140 ksi @Temperature 73.4 °F |
| 8.28 GPa @Temperature 23.0 °C | 1200 ksi @Temperature 73.4 °F |
Compressive Strength | 148 MPa @Temperature 23.0 °C | 21500 psi @Temperature 73.4 °F |
Izod Impact, Notched | 1.33 J/cm @Temperature 23.0 °C | 2.49 ft-lb/in @Temperature 73.4 °F |
Izod Impact, Unnotched | 9.60 J/cm @Temperature 23.0 °C | 18.0 ft-lb/in @Temperature 73.4 °F |
Izod Impact, Notched (ISO) | 13.0 kJ/m² @Temperature 23.0 °C | 6.19 ft-lb/in² @Temperature 73.4 °F |
Charpy Impact Unnotched | 7.00 J/cm² @Temperature 23.0 °C | 33.3 ft-lb/in² @Temperature 73.4 °F |
Charpy Impact, Notched | 1.40 J/cm² @Temperature 23.0 °C | 6.66 ft-lb/in² @Temperature 73.4 °F |
|
Electrical Properties | Metric | English | Comments |
---|
Volume Resistivity | 1.00e+15 ohm-cm @Temperature 23.0 °C | 1.00e+15 ohm-cm @Temperature 73.4 °F |
| 1.00e+15 ohm-cm @Temperature 23.0 °C | 1.00e+15 ohm-cm @Temperature 73.4 °F |
Surface Resistance | 1.00e+14 ohm @Temperature 23.0 °C | 1.00e+14 ohm @Temperature 73.4 °F |
| 1.00e+14 ohm @Temperature 23.0 °C | 1.00e+14 ohm @Temperature 73.4 °F |
Dielectric Constant | 3.3 @Frequency 1e+6 Hz, Temperature 23.0 °C | 3.3 @Frequency 1e+6 Hz, Temperature 73.4 °F |
| 3.3 @Frequency 1e+6 Hz, Temperature 23.0 °C | 3.3 @Frequency 1e+6 Hz, Temperature 73.4 °F |
| 3.4 @Frequency 1000 Hz, Temperature 23.0 °C | 3.4 @Frequency 1000 Hz, Temperature 73.4 °F |
| 4.2 @Frequency 100 Hz, Temperature 23.0 °C | 4.2 @Frequency 100 Hz, Temperature 73.4 °F |
Dielectric Strength | 21.5 kV/mm @Thickness 3.20 mm, Temperature 23.0 °C | 546 kV/in @Thickness 0.126 in, Temperature 73.4 °F |
| 26.5 kV/mm @Thickness 1.60 mm, Temperature 23.0 °C | 673 kV/in @Thickness 0.0630 in, Temperature 73.4 °F |
Dissipation Factor | 0.010 @Frequency 1000 Hz, Temperature 23.0 °C | 0.010 @Frequency 1000 Hz, Temperature 73.4 °F |
| 0.015 @Frequency 1e+6 Hz, Temperature 23.0 °C | 0.015 @Frequency 1e+6 Hz, Temperature 73.4 °F |
| 0.015 @Frequency 1e+6 Hz, Temperature 23.0 °C | 0.015 @Frequency 1e+6 Hz, Temperature 73.4 °F |
Comparative Tracking Index | 325 V @Thickness 3.00 mm, Temperature 23.0 °C | 325 V @Thickness 0.118 in, Temperature 73.4 °F |
|
Thermal Properties | Metric | English | Comments |
---|
CTE, linear, Transverse to Flow | 85.0 µm/m-°C @Temperature -40.0 - 23.0 °C | 47.2 µin/in-°F @Temperature -40.0 - 73.4 °F |
Melting Point | 250 °C | 482 °F |
| 254 °C | 489 °F |
Deflection Temperature at 0.46 MPa (66 psi) | 237 °C | 459 °F |
| 240 °C | 464 °F |
Deflection Temperature at 1.8 MPa (264 psi) | 220 °C | 428 °F |
| 220 °C | 428 °F |
UL RTI, Electrical | 140 °C @Thickness 0.750 mm | 284 °F @Thickness 0.0295 in |
| 140 °C @Thickness 1.50 mm | 284 °F @Thickness 0.0591 in |
| 140 °C @Thickness 3.00 mm | 284 °F @Thickness 0.118 in |
UL RTI, Mechanical with Impact | 140 °C @Thickness 3.00 mm | 284 °F @Thickness 0.118 in |
| 140 °C @Thickness 1.50 mm | 284 °F @Thickness 0.0591 in |
| 140 °C @Thickness 0.750 mm | 284 °F @Thickness 0.0295 in |
UL RTI, Mechanical without Impact | 140 °C @Thickness 3.00 mm | 284 °F @Thickness 0.118 in |
| 140 °C @Thickness 0.750 mm | 284 °F @Thickness 0.0295 in |
| 140 °C @Thickness 1.50 mm | 284 °F @Thickness 0.0591 in |
Flammability, UL94 | HB @Thickness 1.50 mm | HB @Thickness 0.0591 in |
| HB @Thickness 3.00 mm | HB @Thickness 0.118 in |
| HB @Thickness 0.750 mm | HB @Thickness 0.0295 in |
| HB @Thickness 0.750 mm | HB @Thickness 0.0295 in |
| HB @Thickness 1.50 mm | HB @Thickness 0.0591 in |
| HB @Thickness 3.00 mm | HB @Thickness 0.118 in |
Oxygen Index | 22 % | 22 % |
|
Processing Properties | Metric | English | Comments |
---|
Melt Temperature | 280 °C | 536 °F |
| 270 - 290 °C | 518 - 554 °F |
Mold Temperature | >= 95.0 °C | >= 203 °F |
| 110 °C | 230 °F |
Drying Temperature | 120 °C | 248 °F |
Dry Time | 4.00 hour | 4.00 hour |
Moisture Content | <= 0.020 % | <= 0.020 % |
|
Descriptive Properties |
---|
Additive | Impact Modifier |
Appearance | Natural Color |
Drying Recommended | Yes |
Features | Impact Modified |
| Impact Resistance, Good |
| Stiffness, Good |
| Strength, Good |
| Thermal Aging Resistance, Good |
Filler | Glass fiber reinforcement |
Generic | PET |
Heat Stabilized | Yes |
Material Status | Current |
Part Marking Code | >PET-IGF30< |
Polymer Family | Polyester |
Polymer Type | PET |
Processing Method | Injection Molding |
Product Category | Glass Reinforced Resins |
| Toughened Resins |
Resin Identification | PET-IGF30 |
Ultrasonic Weldable | Yes |
Uses | Automotive Applications |
| Housings |
| Structural Parts |