MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Rubidium, Rb
Categories: Metal; Nonferrous Metal; Pure Element

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.45 g/cc
@Temperature 220 °C
 1.46 g/cc
@Temperature 150 °C
 1.47 g/cc
@Temperature 50.0 °C
 1.475 g/cc
@Temperature 39.0 °C
 1.532 g/cc
@Temperature 20.0 °C
Vapor Pressure 0.001333 bar
@Temperature 294 °C
 0.01333 bar
@Temperature 387 °C
 0.1333 bar
@Temperature 519 °C
 0.2666 bar
@Temperature 569 °C
 0.5333 bar
@Temperature 628 °C
Surface Tension 46.8 dynes/cm
@Temperature 632 °C
 51 dynes/cm
@Temperature 550 °C
 80 dynes/cm
@Temperature 100 °C
 84.7 dynes/cm
@Temperature 39.0 °C
 
Chemical PropertiesOriginal ValueComments
Atomic Mass 85.46781995
Atomic Number 37
Thermal Neutron Cross Section 0.70 barns/atom
X-ray Absorption Edge 0.81549 ÅK
 6.006 ÅLI
 6.6538 ÅLII
 6.8752 ÅLIII
Critical Temperature 1820 °C
Electrode Potential -2.90 V
Electronegativity 0.82Pauling
Ionic Radius 1.47 ÅCrystal Ionic Radius for Valence +1
 
Mechanical PropertiesOriginal ValueComments
Modulus of Elasticity 2.35 GPa
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.0000125 ohm-cm
 0.00001154 ohm-cm
@Temperature 0.000 °C
 0.00001284 ohm-cm
@Temperature 20.0 °C
 0.0000137 ohm-cm
@Temperature 39.9 °C
solid
 0.0000220 ohm-cm
@Temperature 39.9 °C
liquid
 0.00002747 ohm-cm
@Temperature 100 °C
liquid
Magnetic Susceptibility 2.0e-7cgs/g
 
Thermal PropertiesOriginal ValueComments
Heat of Fusion 25.5 J/g
Heat of Vaporization 888 J/g
CTE, linear 90.0 µm/m-°C
@Temperature 20.0 °C
Specific Heat Capacity 0.336 J/g-°C
Thermal Conductivity 33.3 W/m-K
@Temperature 38.89 °C
liquid
 58.1 W/m-K
@Temperature 38.89 °C
solid
 58.2 W/m-K
@Temperature 25.0 °C
solid
 58.3 W/m-K
@Temperature 0.000 °C
solid
Melting Point 38.89 °C
Boiling Point 688 °C
 
Component Elements PropertiesOriginal ValueComments
Rubidium, Rb 100 %
 
Descriptive Properties
CAS Number7440-17-7

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Silver, Ag
Aluminum, Al
Cesium, Cs
Potassium, K
Silicon, Si

AMERb00 / 90

New MatWeb Services

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.