MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Titanium Grade 12, Annealed
Categories: Metal; Nonferrous Metal; Titanium Alloy; Unalloyed/Modified Titanium

Material Notes: Addition of 0.3% Mo and 0.8% Ni to titanium increases corrosion resistance at a lower cost than Pd (see Ti Grades 7 and 11). Sample was annealed 20 min. at 815°C and 5 min. at 788°C.

Higher strength than unalloyed Ti grades 1 - 4, yet still formable.

Microstructure: Equiaxed alpha, with acicular alpha, primarily in welds or heat-affected zones, small amounts of beta.

Applications: Chemical processing, in mildly reducing or variable oxidizing-reducing media - containers, heat exchangers, pumps, valves, pipes and fittings.

Forms typically available: billet, bar, rod, plate, sheet, strip and tubing.

Titanium Grades 1,2,3,4,7,11,and 12 are all considered unalloyed and have similar mechanical properties.

Key Words: UNS R53400; ASTM Grade 12, titanium alloy
Vendors: Visit metalmen for your metals needs. Products include special chemistry, tight tolerances, custom tempers, odd dimensions/forms, and small quantities. Phone 1-800-767-9494.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 4.50 g/cc0.163 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength 345 MPa
@Temperature 316 °C
50000 psi
@Temperature 601 °F
Tensile Strength, Ultimate 620 MPa89900 psi
Tensile Strength, Yield 480 MPa69600 psi
Elongation at Break 23 %23 %
Creep Strength 103 MPa
@Temperature 316 °C,
Time >=3.60e+6 sec
14900 psi
@Temperature 601 °F,
Time >=1000 hour
strain 0.3%
Rupture Strength 276 MPa
@Temperature 316 °C,
Time 3.60e+6 sec
40000 psi
@Temperature 601 °F,
Time 1000 hour
Tensile Modulus 103 GPa14900 ksi
Modulus of Rigidity 41.3 GPa5990 ksi
Notched Tensile Strength 620 MPa89900 psiKt (stress concentration factor) = 5.3
Poissons Ratio 0.280.28
Fatigue Strength  140 MPa
@# of Cycles 1.00e+7
20300 psi
@# of Cycles 1.00e+7
Kt (stress concentration factor) = 3.5
 310 MPa
@# of Cycles 1.00e+7
45000 psi
@# of Cycles 1.00e+7
unnotched
Shear Modulus 41.0 GPa5950 ksi
Bend Radius, Minimum 2.5 t
@Thickness >=1.80 mm
2.5 t
@Thickness >=0.0709 in
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.0000520 ohm-cm0.0000520 ohm-cm
 
Thermal PropertiesMetricEnglishComments
Heat of Fusion 325 J/g140 BTU/lbHigh Purity Ti.
CTE, linear  9.50 µm/m-°C
@Temperature 200 °C
5.28 µin/in-°F
@Temperature 392 °F
 9.90 µm/m-°C
@Temperature 20.0 - 93.0 °C
5.50 µin/in-°F
@Temperature 68.0 - 199 °F
 19.9 µm/m-°C
@Temperature 20.0 °C
11.1 µin/in-°F
@Temperature 68.0 °F
perpendicular
Specific Heat Capacity 0.555 J/g-°C0.133 BTU/lb-°F
Thermal Conductivity 19.0 W/m-K132 BTU-in/hr-ft²-°F
Melting Point <= 1660 °C<= 3020 °F
Liquidus 1660 °C3020 °F
Beta Transus 890 °C1630 °F
 
Optical PropertiesMetricEnglishComments
Emissivity (0-1) 0.30
@Temperature 710 °C
0.30
@Temperature 1310 °F
High purity Ti
Reflection Coefficient, Visible (0-1) 0.560.56High purity Ti; visible light.
 
Component Elements PropertiesMetricEnglishComments
Carbon, C <= 0.080 %<= 0.080 %
Hydrogen, H <= 0.015 %<= 0.015 %
Iron, Fe <= 0.30 %<= 0.30 %
Molybdenum, Mo 0.20 - 0.40 %0.20 - 0.40 %
Nickel, Ni 0.60 - 0.90 %0.60 - 0.90 %
Nitrogen, N <= 0.030 %<= 0.030 %
Other, each <= 0.050 %<= 0.050 %
Other, total <= 0.30 %<= 0.30 %
Oxygen, O <= 0.25 %<= 0.25 %
Titanium, Ti 97.725 - 99.2 %97.725 - 99.2 %As Balance; Elemental Composition per ASTM B265

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Titanium Grade 12
Titanium Grade 1
Titanium Grade 1, Annealed
Titanium Grade 2, Annealed
Titanium Grade 7

MTU121 / 14269

Elmet Technologies

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.